Two-phase co-continuous silicon dioxide structure and method for producing the same
By calcining silica and molybdenum compound at high temperature to form an amorphous silica structure composed of Q4 bonds, the alkali resistance and hydrothermal stability of silica-based materials under alkaline conditions and high temperature water vapor are solved. sexual problems reduce harmfulness and achieve complexing with hydrophobic polymers.
Patent Information
- Application Number
- CN202180068858.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-10-09
- Filing Date
- 2021-10-07
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-10-07
AI Technical Summary
Silica-dioxide-based materials have poor alkali resistance and hydrothermal stability when used under alkaline conditions and high temperature water vapor, and crystalline silica is highly harmful and difficult to recombine with hydrophobic polymers.
By mixing silica with molybdenum compound and calcining at high temperature, using molybdenum oxide as a dehydration catalyst for silanol groups, an amorphous silica structure composed of Q4 bond is formed, and the silanol groups are eliminated and a continuous phase is formed. Silicon dioxide network.
It realizes amorphous silica structure with low harmfulness, improves alkali resistance and hydrothermal stability, and can directly compound with hydrophobic polymers, and is suitable for a variety of industrial applications.
Smart Images

Figure BDA0004165730050000131 
Figure BDA0004165730050000141 
Figure HDA0004165730060000011
Abstract
Description
Technical Field
[0001] The present invention relates to a two-phase co-continuous silica structure and a method for producing the structure.
[0002] This application claims priority based on international application No. PCT / JP2020 / 038234 filed in Japan on October 9, 2020, and the contents of which are incorporated herein. Background Art
[0003] Porous materials such as macroporous materials and mesoporous materials have a variety of uses and are used in a wide range of industrial fields such as adsorbents, separation materials, catalyst carriers, resin fillers, battery electrode materials, solid electrolytes, etc. In particular, in terms of diffusion and transportation of substances, due to the requirements of chemical modification in pores, as porous materials, the network-like co-continuous structure in which the skeleton of the three-dimensional network and the cavity tunnel (through hole) are connected and the two phases of the matrix material and the air form a continuous phase with each other has attracted much attention as the next generation of porous materials, and its application in high-functional materials is expected.
[0004] From this background, the synthesis of silica as the skeleton of porous co-continuous structure has attracted much attention. The silica was originally an inorganic material with excellent heat resistance and chemical resistance. As a simple method, it is known that the following method, for example, is used: by heating a mixture of anhydrous silicic acid and an inorganic salt to above the melting point of the inorganic salt, a co-continuous structure based on metastable decomposition is formed, and the inorganic salt is removed to form a porous silica-based co-continuous body (for example, with reference to patent document 1). In addition, it is reported that: by phase separation based on metastable decomposition of a sol-gel reaction with alkoxysilane, a silica-based co-continuous structure with uniform micropores is obtained (for example, with reference to non-patent document 1). Silica gel with this porous structure is widely used as a filler for HPLC columns.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 61-122173
[0008] Patent Document 2: Japanese Patent Application Publication No. 2014-19591
[0009] Non-patent literature
[0010] Nakanishi et al., J. Porous Mater., 1997, 4, 67-112 Summary of the invention
[0011] Problem that the invention aims to solve
[0012] However, there must be a large number of silanol (Si-OH) groups in the chemical structure of silica or silica gel. Therefore, silica-based materials usually have poor alkali resistance and hydrothermal stability and can hardly be used under alkaline conditions or high-temperature water vapor atmospheres. In addition, the silanol groups on the surface of silica or silica gel often bond with water molecules, so the surface shows strong hydrophilicity. Therefore, as long as chemical surface modification is not performed, it is difficult to make silica-based materials directly compound with hydrophobic polymers.
[0013] In order to solve the above problems, a two-phase co-continuous silica structure composed of silica and a cavity and a method for producing the same have been reported, wherein the silica is substantially free of silanol groups and is composed of Q4 bonds (for example, refer to Patent Document 2). However, the two-phase co-continuous silica obtained by the manufacturing method is crystalline silica. It is known that the harmfulness of crystalline silica is very high, and the risk of cancer caused by inhaling dust containing crystalline silica increases. For example, the Japanese Society of Occupational Health regards crystalline silica as a carcinogen classified as the first group "substances that can be judged to be carcinogenic to humans", and in the carcinogenicity classification of the International Agency for Research on Cancer (IARC), it is also classified as "substances observed to be carcinogenic" in Group "1".
[0014] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a two-phase co-continuous silica structure consisting of silica and cavities, and a method for producing the same, wherein the silica contains substantially no silanol groups, has low toxicity, and is composed of Q4 bonds.
[0015] Solutions for solving problems
[0016] The present invention includes the following aspects.
[0017] (1) A two-phase co-continuous silica structure, which consists of a phase with silica as the main component and an air phase, the chemical bonds of the silica are composed of Q4 bonds, the content of molybdenum relative to the total amount of the aforementioned two-phase co-continuous silica structure is less than 2.0 mass%, and the aforementioned phase with silica as the main component is amorphous.
[0018] (2) The two-phase co-continuous silica structure according to (1), wherein the content of the molybdenum compound is 15 mass % or less based on the total amount of the raw materials of the two-phase co-continuous silica structure.
[0019] (3) The two-phase co-continuous silica structure according to (1) or (2), wherein the diameter of the air phase is in the range of 10 to 1000 nm.
[0020] (4) The two-phase co-continuous silica structure according to any one of (1) to (3), wherein the phase containing silica as a main component is formed of nanowires having a thickness in the range of 5 to 1000 nm.
[0021] (5) The two-phase co-continuous silica structure according to any one of (1) to (4), wherein the specific surface area of the two-phase co-continuous silica structure is 0.1 to 200 m 2 / g range.
[0022] (6) The two-phase co-continuous silica structure according to any one of (1) to (5), wherein the phase containing silicon dioxide as a main component of the two-phase co-continuous silica structure contains 5 mass % or less of molybdenum oxide.
[0023] (7) The two-phase co-continuous silica structure according to any one of (1) to (6), which is a spherical particle having a particle diameter of 1 to 100 μm.
[0024] (8) A method for producing a two-phase co-continuous silica structure as described in any one of (1) to (7) above, which comprises the following steps: a step (I) of mixing a precursor silica (X) and a molybdenum compound (Y) to obtain a mixture (A); and a step (II) of heating the mixture (A) obtained in the step (I) in the range of 600 to 1000°C, wherein the content of the molybdenum compound (Y) relative to the total amount of the mixture (A) is 15% by mass or less when converted into molybdenum oxide, and the method comprises: allowing the vapor of molybdenum oxide generated by the heating to function as a dehydration catalyst for silanol, thereby forming a chemical bond of silica by a Q4 bond.
[0025] Effects of the Invention
[0026] According to the present invention, an amorphous two-phase co-continuous silica structure composed of silica and cavities and a method for producing the same can be provided, wherein the silica substantially does not contain a silanol group and is composed of a Q4 bond. The two-phase co-continuous silica structure of the present invention is amorphous and therefore has low toxicity and can be used for various purposes. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the XRD spectrum of the two-phase co-continuous silica structure obtained in each of the Examples and Comparative Examples. DETAILED DESCRIPTION
[0028] In the manufacture of industrial manufacturing or laboratory research of silicon dioxide, all react in the presence of water. Under this condition, the obtained silicon dioxide will inevitably generate a large number of silanol groups. Therefore, in the existing silicon dioxide manufacturing path, it is impossible to give the Q4 structure with a high content. The root of this embodiment is that the silicon dioxide itself obtained by the existing silicon dioxide synthesis method is used as a precursor raw material, and the Si-OH group in the solid state is subjected to a dehydration reaction. For this reason, it is impossible to only use high temperature heating, so the following scheme is considered: using the affinity of the molybdenum compound and silicon dioxide that show high temperature sublimation, the vapor of the metal oxide is infiltrated near the silanol group, and thus, the silicon dioxide is cut (the molybdenum compound functions as a dehydration catalyst of silanol). It is found that the chemical bond of silicon dioxide is composed of Q4 bonds, and the cavity tunnel penetrates from the outer surface of the structure to the internal whole, and the two phases of silicon dioxide and air form a continuous phase with each other.
[0029] In addition, in the present embodiment, it was found that a two-phase co-continuous silica structure in which the phase containing silica as a main component is amorphous is formed by reacting a specific amount of a molybdenum compound with silica under specific temperature conditions.
[0030] It should be noted that the two-phase co-continuous silica structure in the present embodiment may contain a small amount of molybdenum oxide that is not completely sublimated and remains on the surface of the silica. In this sense, "with ... as the main component" means that more than 85% by mass of the solid part forming the structure is silica, preferably more than 90% by mass is silica. The present invention is described in detail below.
[0031] [Precursor silicon dioxide (X)]
[0032] In this embodiment, the silica used as the precursor is not particularly limited as long as it is amorphous silica, and for example, synthetic silica-based materials such as silica gel, silica nanoparticles, and mesoporous silica, or silica existing in nature such as biosilica, etc. can be used.
[0033] The specific surface area of the precursor silica (X) is not particularly limited, but is preferably 10 m2 from the viewpoint of being able to easily form an air phase in the form of a continuous body (through pores). 2 / g or more, more preferably 100m 2 / g or above.
[0034] The shape of the precursor silica (X) is also not particularly limited. Since the overall shape of the micrometer size or more is maintained as it is, a two-layer co-continuous silica structure can be formed. Therefore, it is preferred to select a precursor silica (X) of an appropriate shape according to the purpose. For example, a spherical, irregularly shaped (shapeless), a structure (lead, fiber, belt, tube, etc.) with a planar shape (aspect), a sheet, etc. can be suitably used.
[0035] The overall size of the precursor silica (X) is also not particularly limited. For example, when silica particles with a micron size or larger are used, a co-continuous silica structure can be formed while maintaining the size of one particle itself, and when silica particles with a small particle size are used, multiple particles can be fused to form a large co-continuous silica structure.
[0036] In addition, the precursor silica (X) may be composed of only silica, or may be a composite of silica and an organic compound. For example, even an organic / inorganic composite obtained by modifying silica using an organosilane, a composite silica adsorbed with a polymer, etc., may be suitably used. The content of the organic compound when using these composites is not particularly limited, but from the viewpoint of effectively manufacturing a two-phase co-continuous silica structure, the content is preferably 60% by mass or less, more preferably 30% by mass or less.
[0037] [Molybdenum compound (Y)]
[0038] In this embodiment, in order to form a silicon dioxide structure composed of Q4 bonds, a molybdenum compound (Y) must be used. The molybdenum compound may be molybdenum oxide or an acid anion (MO) formed by a bond between molybdenum metal and oxygen. x n- ) compounds.
[0039] As the aforementioned acid anion (MO x n- ) is not particularly limited as long as it can be converted into molybdenum oxide by high-temperature calcination. For example, molybdic acid, H 3 PMo 12 O 40 , H 3 SiMo 12 O 40 NH 4 Mo 7 O 12 Etc. Among these, in consideration of cost, it is preferable to use molybdenum oxide as it is.
[0040] [Mixing and calcination]
[0041] The present embodiment is characterized in that a two-phase co-continuous silica structure consisting of a phase with silica as a main component and an air phase is formed by mixing a precursor silica (X) with a molybdenum compound and calcining the mixture (A), wherein the silanol group of the silica substantially disappears and is composed of Q4 bonds.
[0042] As the charging ratio of the above-mentioned mixture (A), the molybdenum compound (Y) is preferably 15% by mass or less, more preferably in the range of 1 to 15% by mass, further preferably in the range of 1.5 to 10% by mass, and further preferably in the range of 3 to 10% by mass, relative to the precursor silicon dioxide (X). By making the amount of the molybdenum compound (Y) within the above-mentioned preferred range, the phase with silicon dioxide as the main component is easy to form amorphous, and the formation of a two-phase co-continuous silicon dioxide structure is easy and effective.
[0043] The process for preparing the mixture (A) is not particularly limited, and may be, for example, dry mixing without using a solvent or wet mixing with the aid of a solvent.
[0044] The calcination temperature may be any temperature at which molybdenum oxide sublimates, specifically, preferably 600 to 1000° C., more preferably 700 to 1000° C., and even more preferably 800 to 1000° C. If the calcination temperature is within the preferred range, the phase with silicon dioxide as the main component is easily amorphous, and the formation of a two-phase co-continuous silicon dioxide structure is easily and efficiently performed.
[0045] Regarding the charging ratio of the above-mentioned mixture (A), when the molybdenum compound (Y) is 1 to 5 mass % relative to the precursor silicon dioxide (X), the above-mentioned calcination temperature is preferably in the range of 600 to 1000°C, more preferably in the range of 700 to 1000°C, and further preferably in the range of 800 to 1000°C.
[0046] Regarding the charging ratio of the above-mentioned mixture (A), when the molybdenum compound (Y) exceeds 5 mass % and is less than 15 mass % relative to the precursor silicon dioxide (X), the above-mentioned calcination temperature is preferably in the range of 600 to 900°C, more preferably in the range of 700 to 900°C, and further preferably in the range of 800 to 900°C.
[0047] The calcination atmosphere is not particularly limited as long as oxygen is present, but an air atmosphere is more preferred in consideration of safety and cost.
[0048] [Two-phase co-continuous silica structure]
[0049] By calcining a mixture (A) of precursor silica (X) and a molybdenum compound (Y) in the range of 600 to 1000°C, molybdenum oxide forms an attached film on the surface of the pores of the precursor silica (X). If the silica with an attached film on the surface is further calcined at a high temperature, the silanol groups in the silica substantially disappear while the molybdenum oxide sublimates, forming a two-phase co-continuous silica structure of nano-sized cavities that are continuous (through) as a whole of the silica structure and a three-dimensional network skeleton of silica composed of Q4 bonds. That is, it can be considered that during high-temperature calcination, molybdenum oxide functions as a dehydration reaction catalyst of the silanol group. At this time, by selecting the ratio of the precursor silica (X) to the molybdenum compound, the calcination temperature, or the pore properties of the precursor silica (X) (pore size, distribution, etc.), the chemical properties and nanostructure of the desired two-phase co-continuous silica structure can be controlled.
[0050] In the two-phase co-continuous silica structure of the present embodiment, the phase with silica as the main component is amorphous. That is, the two-phase co-continuous silica structure of the present embodiment does not substantially contain crystalline silica. Therefore, the two-phase co-continuous silica structure of the present embodiment has low toxicity and can be used for various purposes.
[0051] In the two-phase co-continuous silica structure of the present embodiment, the content of molybdenum relative to the total amount of the two-phase co-continuous silica structure is 2.0 mass % or less. By appropriately selecting the charging ratio of the above-mentioned mixture (A) in such a manner that the content of molybdenum relative to the total amount of the two-phase co-continuous silica structure becomes 2.0 mass % or less, a two-phase co-continuous silica structure having silica as the main component and an amorphous phase is obtained.
[0052] The content of molybdenum relative to the total amount of the two-phase co-continuous silica structure is preferably in the range of 0.5 to 1.9 mass %, more preferably in the range of 0.5 to 1.8 mass %, and further preferably in the range of 0.5 to 1.8 mass %. If the content of molybdenum relative to the total amount of the two-phase co-continuous silica structure is within the above-mentioned preferred range, it is easy to more reliably obtain a two-phase co-continuous silica structure in which the phase with silicon dioxide as the main component is amorphous.
[0053] The diameter of the air phase in the two-phase co-continuous silica structure of the present embodiment is preferably in the range of 10 to 1000 nm, especially in the range of 50 to 1000 nm. The diameter of the cavity tunnel (air phase) in the two-phase co-continuous silica structure can be increased by increasing the calcination temperature or the content of the molybdenum compound (Y) in the mixture (A), or by using a precursor silica (X) having a higher specific surface area.
[0054] The silica network in the two-phase co-continuous silica structure of this embodiment uses nanowires as the basic structure, which forms a three-dimensional network. The thickness of the nanowires is in the range of 5 to 1000 nm, and is particularly suitable for obtaining materials in the range of 30 to 500 nm. By increasing the calcination temperature or increasing the content of the molybdenum compound in the mixture (A), or using a precursor silica (X) with a higher specific surface area, the thickness of the nanowire-shaped silica in the two-phase co-continuous silica structure can be thickened.
[0055] Compared with the precursor silica (X), the specific surface area of the obtained two-phase co-continuous silica structure is greatly reduced. It also depends on the properties of the precursor silica (X) and the calcination conditions. The specific surface area of the obtained two-phase co-continuous silica structure is 0.1 to 200 m 2 / g range, suitable for obtaining 0.1~50m 2 / g range of substances.
[0056] By high temperature calcination treatment, the molybdenum compound used is mostly sublimated to form a silicon dioxide structure with silicon dioxide as the main component. However, the two-phase co-continuous silicon dioxide structure sometimes contains a small amount of molybdenum oxide that is not sublimated cleanly. Their content is less than 5% by mass, and in particular, their content can be made less than 1% by mass by sufficient calcination time and calcination temperature.
[0057] The shape of the two-phase co-continuous silica structure described in this embodiment is not particularly limited, and can be spherical particles with a particle size of 1 to 500 μm, preferably 1 to 100 μm, and more preferably 1 to 60 μm. If the two-phase co-continuous silica structure is a spherical particle with a particle size of 1 to 60 μm, it is easy to synthesize the two-phase co-continuous structure while maintaining the particle shape.
[0058] In this specification, the particle size of the two-phase co-continuous silica structure is measured by using a laser diffraction particle size distribution meter HELOS (H3355) & RODOS, R3: 0.5 / 0.9-175 μm (manufactured by Nippon Laser Co., Ltd.) under dry conditions of a dispersion pressure of 3 bar and an induction pressure of 90 mbar.
[0059] In the present embodiment, when the two-phase co-continuous silica structure is a spherical particle, the circularity of the spherical particle is preferably 0.7 or more, and more preferably 0.75 or more.
[0060] In this specification, the circularity is calculated from SEM images of 900 or more particles using the fully automatic image analysis service "DeepCle" (Sakai Chemical Industry Co., Ltd.) Model 872, and the average value is used.
[0061] The molybdenum oxide in the two-phase co-continuous silica structure forms an amorphous structure on the outer surface and inside of the silica. These oxides can be removed by washing with an aqueous ammonia solution or an aqueous sodium hydroxide solution.
[0062] Molybdenum oxide functions as a dehydration catalyst at high temperatures to form a two-phase co-continuous silica structure, the bonding state of which can be 29 The three-dimensional silica network in the two-phase co-continuous silica structure is different from ordinary silica and has a structure formed by Q4 bonds, similar to silica in quartz glass.
[0063] There are a lot of silanol groups in common silica gel, so the alkali resistance is very weak. In contrast, the two-phase co-continuous silica structure of the present embodiment does not have silanol groups substantially, so it shows excellent alkali resistance. For example, in a sodium hydroxide aqueous solution of less than 0.1 mol / L, no hydrolysis is observed even if it is placed at room temperature (25-30°C) for 1 month, and the two-phase co-continuous structure can be maintained in the initial state.
[0064] In addition, in a high concentration sodium hydroxide aqueous solution of 0.1 mol / L or more, the surface of the silica wires in the two-phase co-continuous silica structure is etched, and the thickness of the wires, the basic structure of the silica network, can be reduced while maintaining the shape of the co-continuum.
[0065] In addition, the structure of the present embodiment has substantially no silanol groups, and thus the polarity of the surface of the structure is greatly reduced. Therefore, the water vapor adsorption of the two-phase co-continuous silica structure becomes much lower than that of the precursor silica (X).
[0066] By having this property, the two-phase co-continuous silica structure of the present embodiment can be suitably used as a resin filler. That is, common silica has a high surface polarity derived from the surface silanol group, so when used as a filler for general polymers, it is difficult to mix evenly as long as surface modification is not performed. In contrast, the silica structure composed of the Q4 structure described in the present embodiment can be directly used as a filler. For example, in a composite of a two-phase co-continuous silica structure and polymethyl methacrylate (PMMA), PMMA diffuses into the entire through cavity (air phase), and can form a very uniform and thin film on the surface of the nanowire, i.e., the basic structure of silica.
[0067] In addition, the two-phase co-continuous silica structure of the present embodiment is mechanically fragile, so even if the initial size is several millimeters or more, it can be easily crushed to a powder of several nanometers using a dispersing device. Therefore, when it is used as a filler, the dispersibility in the resin is improved, which is effective in improving the transparency of the obtained resin molded body.
[0068] Example
[0069] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to these examples. It should be noted that "%" means "mass %" unless otherwise specified.
[0070] [Analysis based on X-ray diffraction]
[0071] The prepared sample is placed on a 0.5 mm deep measurement sample holder, filled with a specified load to make it flat, and placed on a wide-angle X-ray diffraction (XRD) device such as Ultima IV manufactured by Rigaku Corporation, and measured under the conditions of Cu / Kα rays, 40 kV / 40 mA, a scanning speed of 2 degrees / minute, and a scanning range of 10 to 70 degrees.
[0072] [Composition analysis of nanostructures of two-phase co-continuous structures using fluorescent X-rays]
[0073] Using a fluorescent X-ray (XRF) analyzer Primus IV (manufactured by Rigaku Corporation), about 70 mg of the prepared sample was placed on filter paper, covered with a PP film, and subjected to composition analysis.
[0074] [Shapter analysis of the shape of two-phase co-continuous silica structures using scanning electron microscopy]
[0075] The sample was fixed to a sample support table with a double-sided tape, and observed using a surface observation device VE-9800 manufactured by KEYENCE Corporation.
[0076] [Nanostructural analysis of two-phase co-continuous silica structure using transmission electron microscopy]
[0077] The sample prepared as a cross section was placed on a carbon-evaporated copper grid and observed using an EM-002B or VOYAGER M3055 high-resolution electron microscope manufactured by TOPCON or NOLAN INSTRUMENT.
[0078] [based on 29 Evaluation of chemical bonds in two-phase co-continuous silica structures measured by Si CP / MAS NMR]
[0079] 29Si CP / MAS NMR measurement was performed using JEOL JNM-ECA600. As a reference for chemical shift, polydimethylsilane was separately measured by CP / MAS method, and the obtained peak was set to -33.8 ppm.
[0080] [Measurement of particle size]
[0081] The measurement was performed using a laser diffraction particle size distribution analyzer HELOS (H3355) & RODOS, R3: 0.5 / 0.9-175 μm (manufactured by Nippon Laser Technology Co., Ltd.) under dry conditions with a dispersion pressure of 3 bar and an input pressure of 90 mbar.
[0082] [Measurement of circularity]
[0083] The circularity of more than 900 particles was calculated from the SEM images using the fully automatic image analysis service "DeepCle" (Sakai Chemical Industry Co., Ltd.), model 872, and the average value was used.
[0084] [Calcination method]
[0085] The calcination was performed using a calcination furnace apparatus equipped with an AMF-2P type temperature controller in a ceramic electric tubular furnace ARF-100K type manufactured by Asahi Rika Seisakusho Co., Ltd.
[0086] (Example 1)
[0087] <Preparation and Calcination of a Mixture of Silica Gel and Molybdenum Oxide>
[0088] 20 g of silica gel (manufactured by Kanto Chemical Co., Ltd., silica gel 60, spherical, average particle size of 40 to 50 μm) and 1 g of molybdenum oxide (manufactured by Wako Co., Ltd.) were mixed in a mortar to obtain 21 g of a mixture (A-1) of precursor silica and molybdenum oxide. 21 g of the obtained mixture (A-1) was calcined at 8000°C for 5 hours in an electric furnace. Most of the molybdenum oxide was sublimated to obtain about 18.2 g of white powder. Next, 18.2 g of the obtained white powder was dispersed in 150 mL of 0.25% ammonia water, and the dispersed solution was stirred at room temperature (25 to 30°C) for 3 hours, and then the ammonia water was removed by filtration, and the particles were washed with water and dried to remove the molybdenum remaining on the surface of the particles, thereby obtaining 17.3 g of powder of a silica structure. It was confirmed by SEM and TEM observation that the obtained silica structure was a two-phase co-continuous structure in which cavity tunnels penetrated from the outer surface to the entire interior, and the two phases of silica and air formed a continuous phase with each other.
[0089] The powder of the two-phase co-continuous silica structure obtained above was used to 29In Si CP / MAS NMR measurement, no peaks derived from Q2, Q3, and Q4 were observed in the range of 80 ppm to 120 ppm. This suggests that the silanol groups in the silica structure completely disappeared after molybdenum oxide treatment, and the resulting silica structure was similar to quartz glass having only Q4 bonds.
[0090] Furthermore, the crystallinity of the obtained two-phase co-continuous silica structure was analyzed by X-ray diffraction, and it was confirmed that the two-phase co-continuous silica structure was amorphous.
[0091] Furthermore, the amount of molybdenum remaining in the obtained two-phase co-continuous silica structure was analyzed by fluorescent X-ray measurement. As a result, it was confirmed that the amount of molybdenum in the two-phase co-continuous silica structure was 1.23%.
[0092] (Examples 2 to 10, Comparative Examples 1 to 4)
[0093] The two-phase co-continuous silica structure was obtained in the same manner as in Example 1 except that the amount of raw materials, average particle size, calcination temperature and calcination time were changed to the conditions shown in Table 1. SEM and TEM observations confirmed that the obtained silica structure was a two-phase co-continuous structure in which cavity tunnels penetrated from the outer surface to the entire interior, and the two phases of silica and air formed a continuous phase with each other.
[0094] The powders of the two-phase co-continuous silica structures obtained in Examples 2 to 10 and Comparative Examples 1 to 4 were used to perform 29 In Si CP / MAS NMR measurement, no peaks derived from Q2, Q3, and Q4 were observed in the range of 80 ppm to 120 ppm.
[0095] In addition, the crystallinity and the amount of residual molybdenum of the two-phase co-continuous silica structures obtained in Examples 2 to 10 and Comparative Examples 1 to 4 were analyzed in the same manner as in Example 1. The results are shown in Table 1.
[0096] [Table 1]
[0097]
[0098] [Table 2]
[0099]
[0100] In the table, evaluation of crystallinity is as follows.
[0101] A: The phase containing silicon dioxide as the main component has an amorphous structure.
[0102] A+C: The phase containing silicon dioxide as the main component has an amorphous structure and a crystalline structure.
[0103] C: The phase having silicon dioxide as the main component is a crystal structure.
[0104] In addition, the XRD spectra of the two-phase co-continuous silica structures obtained in each of the Examples and Comparative Examples are shown in Figure 1 .
[0105] According to Table 1 and Figure 1 The results shown confirmed that the residual amount of molybdenum in the two-phase co-continuous silica structure of Examples 1 to 10 was 2.0 mass % or less, and that the phase containing silica as the main component was an amorphous structure.
[0106] The preferred embodiments of the present invention are described above, but the present invention is not limited to these embodiments. Features may be added, omitted, replaced, and otherwise modified without departing from the spirit of the present invention. The present invention is not limited by the foregoing description, but only by the scope of the appended claims.
Claims
1. A two-phase co-continuous silica structure, which consists of a phase with silica as the main component and an air phase, The chemical bonds of this silicon dioxide are composed of Q4 bonds. The content of molybdenum relative to the total amount of the two-phase co-continuous silica structure is 2.0 mass % or less, The phase with silicon dioxide as the main component is amorphous, The diameter of the air phase is in the range of 50 to 1000 nm. The two-phase co-continuous silica structure does not substantially contain crystalline silica.
2. The two-phase co-continuous silica structure according to claim 1, wherein: The phase containing silicon dioxide as a main component has nanowires with a thickness ranging from 5 to 1000 nm as a basic structure and forms a three-dimensional network.
3. The two-phase co-continuous silica structure according to claim 1, wherein: The specific surface area of the two-phase co-continuous silica structure is 0.1 to 200 m 2 / g range.
4. The two-phase co-continuous silica structure according to claim 1, wherein: In the two-phase co-continuous silica structure, the phase containing silicon dioxide as a main component contains 5 mass % or less of molybdenum oxide. 5 . The two-phase co-continuous silica structure according to claim 1 , which is a spherical particle having a particle diameter of 1 to 100 μm.
6. The method for producing a two-phase co-continuous silica structure according to any one of claims 1 to 5, comprising the following steps: A step (I) of mixing a precursor silicon dioxide (X) and a molybdenum compound (Y) to obtain a mixture (A); and a step (II) of heating the mixture (A) obtained in the step (I) at a temperature in the range of 600 to 1000° C., In the mixture (A), the content of the molybdenum compound (Y) is 1 to 5% by mass in terms of molybdenum oxide relative to the total amount of the precursor silicon dioxide (X). The manufacturing method comprises: The vapor of molybdenum oxide generated by the heating functions as a dehydration catalyst of silanol, thereby forming a chemical bond of silicon dioxide by a Q4 bond.
7. The method for producing a two-phase co-continuous silica structure according to any one of claims 1 to 5, comprising the following steps: A step (I) of mixing a precursor silicon dioxide (X) and a molybdenum compound (Y) to obtain a mixture (A); and a step (II) of heating the mixture (A) obtained in the step (I) at a temperature in the range of 600 to 900° C., In the mixture (A), the content of the molybdenum compound (Y) relative to the total amount of the precursor silicon dioxide (X) is more than 5% by weight and less than 15% by weight in terms of molybdenum oxide, The manufacturing method comprises: The vapor of molybdenum oxide generated by the heating functions as a dehydration catalyst of silanol, thereby forming a chemical bond of silicon dioxide by a Q4 bond.