A liquid sunlight zero-carbon emission methanol synthesis catalyst and its preparation method and application
By introducing third and fourth group metal elements into the ZnZr catalyst, the catalyst was prepared by co-precipitation and combined with renewable energy electrolysis of water to produce hydrogen, which solved the problem of carbon dioxide emissions in traditional coal chemical industry and achieved efficient zero-carbon emission methanol synthesis.
Patent Information
- Application Number
- CN202111538826.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-15
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-12-15
AI Technical Summary
Existing industrial methanol production processes generate significant carbon dioxide emissions, and traditional coal chemical processes are complex and require high fixed asset investments, making it difficult to achieve zero carbon emissions.
Based on ZnZr, third and fourth group metal elements are introduced, and the Y/Zr molar ratio is precisely controlled. A co-precipitation method is used to prepare a catalyst, which is then combined with renewable energy water electrolysis to produce hydrogen and integrated into traditional coal chemical processes to prepare a liquid solar-powered zero-carbon emission methanol synthesis catalyst.
The catalyst achieves uniform dispersion of active components, efficiently converts CO and CO2 into methanol, reduces byproducts, exhibits good catalyst stability, is suitable for large-scale application, and realizes zero-carbon emission methanol synthesis.
Smart Images

Figure GDA0003566090420000091 
Figure GDA0003566090420000092 
Figure GDA0003566090420000101
Abstract
Description
Technical Field
[0001] The present application belongs to the field of zero-carbon emission methanol synthesis catalysts, and specifically relates to a liquid sunlight zero-carbon emission methanol synthesis catalyst, a preparation method and an application thereof. Background Art
[0002] Modern coal chemical industry is an important direction of coal utilization. It mainly obtains synthesis gas through coal gasification, and then synthesizes various liquid fuels and chemicals. This process produces a large amount of carbon dioxide.
[0003] At present, industrial methanol production is mainly based on synthesis gas, and the raw materials mainly come from coal gasification, natural gas, petroleum fuels, etc. After gasification, conversion, low-temperature methanol washing and purification, H2, CO2, and CO synthesis gas are synthesized. The excess CO2 is discharged during the low-temperature methanol washing process to meet the operation of industrial methanol. The production of one ton of methanol emits nearly 3.0 tons of carbon dioxide. Under the goal of carbon neutrality, we propose a zero-carbon emission synthetic methanol optimized for industrial production such as coal chemical industry, namely liquid sunlight technology, which uses large-scale renewable energy such as solar energy / wind energy / hydropower to generate electricity, and then electrolyzes water to produce green hydrogen, which is integrated and coupled with the traditional coal chemical methanol production process, and uses electrolysis of water to produce hydrogen instead of water vapor conversion hydrogen production in traditional coal chemical industry, thereby achieving zero-carbon emission methanol synthesis. Not only does it shorten the chemical process flow and reduce fixed asset investment, it also creatively introduces renewable energy to generate hydrogen, realizes integrated coupling with traditional coal chemical industry and other methanol production processes, and fundamentally avoids carbon dioxide emissions. Summary of the invention
[0004] Based on ZnZr, the present application introduces a certain proportion of the third component and the fourth component (metal elements of the IIIA group), and then accurately controls the Y (Y = Al, Ga, In) / Zr molar ratio, adds the ZnZr-X (X = Cu, Pd) Y (Y = Al, Ga, In) salt solution to the precipitant solution for precipitation, and reversely drips the salt solution into the precipitant aqueous solution under the condition of controlling a certain drop rate, and performs precipitation reaction in 50-80°C water, and strictly controls the pH of the drop end point to be 6-8. This co-precipitation in an alkaline atmosphere to prepare the catalyst allows the zinc salt and the precipitant to fully react, ensuring that the molar ratio of the catalyst metal salt is basically consistent with the molar ratio of the experimental design, ensuring the activity of the catalyst, and the process is simple and the preparation cycle is short. Adding Cu (Pd) is more conducive to hydrogen activation, adding the metal element Y (Y = Al, Ga, In) of the IIIA group as an auxiliary, accurately controlling the Y (Y = Al, Ga, In) / Zr molar ratio, promoting the dispersion of each component in the catalyst, and improving the activity of the catalyst. This series of catalysts has good stability during long-term operation.
[0005] According to one aspect of the present application, a liquid sunlight zero-carbon emission methanol synthesis catalyst comprises an oxide solid solution;
[0006] The oxides include zinc oxide, zirconium oxide, oxides of element X and oxides of element Y;
[0007] The element X oxide is selected from copper oxide or palladium oxide;
[0008] The oxide of the element Y is selected from the oxides of metal elements of Group IIIA, such as aluminum oxide, gallium oxide or indium oxide;
[0009] The ratio of the sum of the molar amount of zinc in the zinc oxide and the molar amount of zirconium in the zirconium oxide to the sum of the molar amount of element X in the oxide of element X and the molar amount of element Y in the oxide of element Y is 1:6 to 6:1;
[0010] The ratio of the molar amount of element X in the oxide of element X to the molar amount of element Y in the oxide of element Y is 1:7 to 7:1.
[0011] The sum of the molar amount of the element X in the oxide of the element X and the molar amount of the element Y in the oxide of the element Y accounts for 40-60% of the sum of the molar amount of zinc in the zinc oxide and the molar amount of zirconium in the zirconium oxide.
[0012] The specific surface area of the catalyst microstructure is 60 to 150 m 2 / g, empty volume 0.2~0.6cm 3 / g, pore size 4~30nm;
[0013] According to another aspect of the present application, a method for preparing the above-mentioned liquid sunlight zero-carbon emission methanol synthesis catalyst is provided, comprising at least the following steps:
[0014] (1) mixing raw materials containing a zinc source, a zirconium source, an element X source, and an element Y source with deionized water to obtain a metal salt mixed solution;
[0015] (2) adding a precipitant to deionized water and mixing and stirring to obtain a precipitant solution;
[0016] (3) The metal salt mixed solution obtained in (1) is added dropwise to the precipitant solution obtained in (2) at a certain temperature and stirring rate for precipitation reaction, and the catalyst for liquid sunlight zero-carbon emission methanol synthesis is obtained after aging, water washing, drying and roasting.
[0017] (1), wherein the zinc source is selected from at least one of zinc nitrate and zinc acetate;
[0018] The zirconium source is selected from at least one of zirconium nitrate or zirconium oxynitrate;
[0019] When the element X is copper, the source of the element X is selected from at least one of copper nitrate or acetate;
[0020] When the element X is palladium, the source of the element X is selected from at least one of palladium nitrate or palladium chloride;
[0021] When the element Y is gallium or indium, the source of the element Y is selected from nitrates;
[0022] When the element Y is aluminum, the source of the element Y is selected from at least one of aluminum nitrates and aluminum acetates.
[0023] The usage amount of the zinc source, zirconium source, element X source and element Y source (Zn+Zr) / (X(X=Cu, Pd)+Y(Y=Al, Ga, In)) is 1:2 to 2:1.
[0024] In the mixed solution, the total concentration of the zinc source, the zirconium source, the element X source and the element Y source is 0.3-0.8 mol / L.
[0025] (2), the precipitant is selected from at least one of sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, sodium hydroxide or potassium hydroxide;
[0026] The concentration of the precipitant in the precipitant solution is 0.3-0.8 mol / L;
[0027] In (3), the amount of the metal salt mixed solution obtained in (1) and the precipitant solution obtained in (2) is 1:1 to 1:1.2.
[0028] The reverse dropwise precipitation is to dropwise add the metal salt mixed solution obtained in (1) into the precipitant solution obtained in (2);
[0029] The dropping speed is 5-10 ml / min;
[0030] The pH at the end point of the dropwise addition is 6 to 8;
[0031] The reaction temperature is 50-80°C;
[0032] The reaction time is 2 to 8 hours;
[0033] The aging time after the precipitation reaction is 2 to 8 hours;
[0034] The calcination temperature is 350-450°C;
[0035] The calcination time is 3 to 8 hours;
[0036] The method is also dried before roasting;
[0037] The drying temperature is 60-120°C;
[0038] The drying time is 6 to 15 hours.
[0039] According to another aspect of the present application, a method for synthesizing liquid sunlight zero-carbon emission methanol is provided, comprising at least the following steps:
[0040] A mixed gas containing carbon monoxide, carbon dioxide and hydrogen is in contact with a catalyst under certain reaction conditions, and a catalytic reaction occurs to obtain a product containing methanol;
[0041] The catalyst is selected from the above-mentioned liquid sunlight zero-carbon emission methanol synthesis catalyst or the liquid sunlight zero-carbon emission methanol synthesis catalyst prepared by the above-mentioned preparation method.
[0042] The catalyst is pre-treated;
[0043] The pre-treatment process at least comprises the following steps:
[0044] In an activation atmosphere, treat at a temperature of 200 to 300°C for 2 to 24 hours;
[0045] The pressure of the activation atmosphere is 0.1-1 MPa;
[0046] The activation atmosphere is selected from a mixed gas of hydrogen and an inert gas;
[0047] The inert gas is selected from at least one of helium, argon or nitrogen;
[0048] The volume concentration of hydrogen in the activation atmosphere is 5 to 99.999%.
[0049] The gas pressure of the raw material is 2-10 MPa;
[0050] The feed space velocity of the raw material is 4000~20000h –1 ;
[0051] The molar ratio of the sum of carbon monoxide and carbon dioxide in the raw material to hydrogen is 1:2 to 1:3;
[0052] The temperature of the catalytic reaction is 180-280°C;
[0053] The process is carried out in a fixed bed reactor.
[0054] The beneficial effects of this application are:
[0055] The active components of the liquid sunlight zero-carbon emission methanol synthesis catalyst are evenly dispersed, the catalyst strength is high, and it can efficiently realize the co-hydrogenation of CO and CO2 into methanol, with few by-products and good stability. This series of catalysts is simple to prepare and suitable for large-scale preparation. It can be used to couple renewable energy hydrogen production with optimization of coal chemical industry and other chemical industries, synthesize liquid sunlight methanol, and realize zero-carbon emission methanol synthesis. DETAILED DESCRIPTION
[0056] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0057] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0058] The activity of the catalyst for the co-hydrogenation of CO and CO2 to methanol was evaluated on a fixed bed reactor-GC system. The reaction was carried out at 2-10 MPa, 180-280°C, and the composition of the raw synthesis gas was n(H2):n(CO x ) molar ratio = 1:2 ~ 1:3, space velocity GHSV = 4000 ~ 20000mL / (hg) reaction conditions. Before the reaction, the oxide catalyst is activated at normal pressure, pure hydrogen or a mixture of hydrogen and inert gas at 250 ° C for 2h, then adjusted to the required temperature for the reaction, and switched to introduce raw gas. The tail gas discharged from the reactor outlet is discharged to normal pressure through a back pressure valve, and sampled through a gas chromatography ten-way valve at 150 ° C, and analyzed online by a thermal conductivity detector (TCD) and a hydrogen flame detector (FID) of an Agilent GC-7890B gas chromatograph. The former chromatographic column is a 5A molecular sieve combined with Propark Q (Agilent), with a column length of 3m, using H2 as the carrier gas, working at 90°C, and is used to separate and detect CO2, Ar, and CO; the latter chromatographic column is a TG-BOND Q capillary column (Thermo Fisher Scientific), with a specification of 30m×0.32mm×10μm, using N2 as the carrier gas, and is used to separate and detect low-carbon hydrocarbons and alcohols.
[0059] The CO and CO2 conversion rates and the C-group selectivity and time-space yields of carbon-containing products such as CO2, alcohols, and hydrocarbons were calculated by the C-group internal standard method.
[0060] Example 1
[0061] Weigh 12mmol Zn(NO3)2·6H2O, 8mmol Zr(NO3)4·5H2O, 2mmol Ga(NO3)3·xH2O, 30mmol Cu(NO3)2·3H2O, and prepare 104mL metal salt solution; weigh 62.4mmol Na2CO3 and prepare 125mL Na2CO3 aqueous solution in a 500mL four-necked beaker; insert a pH meter and a thermometer, drip the metal salt solution into the Na2CO3 aqueous solution at 70°C, and drip in reverse to cause precipitation reaction; stir at 600r / min, precipitation rate 6mL / min, control pH=7.0; age at 70°C for 2h; filter after aging, wash with deionized water 5 times until there is no sodium ion in the filtrate; dry the filter cake at 100°C, and calcine in air at 450°C for 4h to obtain the catalyst. Press the tablets at 20MPa, crush, and screen 40-80 mesh for evaluation.
[0062] 1.0 g of the screened catalyst was weighed and loaded into a reaction tube with an inner diameter of 6 mm. It was reduced in pure H2 at 250°C under normal pressure for 2 h with a flow rate of 20 mL / min. Then, raw gas n(H2):n(CO2):n(CO):n(Ar)=67:8.2:21.2:4 was introduced. The reaction was carried out under the conditions of 2 MPa, 240°C, and GHSV=8000 mL / (hg). The detailed results are shown in Table 1.
[0063] Example 2
[0064] Weigh 12mmol Zn(NO3)2·6H2O, 8mmol Zr(NO3)4·5H2O, 4mmol Ga(NO3)3·xH2O, and 30mmol Cu(NO3)2·3H2O to prepare 108mL of metal salt solution; weigh 64.8mmol Na2CO3 to prepare 130mL of aqueous solution and place it in a 500mL four-necked beaker; insert a pH meter and a thermometer, and drip the metal salt solution into the Na2CO3 aqueous solution at 70°C, and drip in the reverse direction to cause a precipitation reaction. The other steps are the same as in Example 1, and the detailed results are shown in Table 1.
[0065] Example 3
[0066] 15mmol Zn(NO3)2·6H2O, 30mmol Zr(NO3)4·5H2O, 4mmol Ga(NO3)3·xH2O were weighed to prepare 100mL metal salt solution, and 1mmol PdCl2 hydrochloric acid solution was added to the ZnZrGa salt solution; 60mmol Na2CO3 was weighed to prepare 120mL aqueous solution and placed in a 500mL four-necked beaker; a pH meter and a thermometer were inserted, and the metal salt solution was dripped into the Na2CO3 aqueous solution at 70°C, and the precipitation reaction occurred in reverse dripping. The other steps were the same as in Example 1, and the detailed results are shown in Table 1.
[0067] Example 4
[0068] 15mmol Zn(NO3)2·6H2O, 28mmol Zr(NO3)4·5H2O, 6mmol Ga(NO3)3·xH2O were weighed to prepare 100mL metal salt solution, and 1mmol PdCl2 hydrochloric acid solution was added to the ZnZrGa salt solution; 60mmol Na2CO3 was weighed to prepare 120mL aqueous solution and placed in a 500mL four-necked beaker; a pH meter and a thermometer were inserted, and the metal salt solution was dripped into the Na2CO3 aqueous solution at 70°C, and the precipitation reaction occurred by reverse dripping. The other steps were the same as in Example 1, and the detailed results are shown in Table 1.
[0069] Example 5
[0070] Weigh 14.5mmol Zn(NO3)2·6H2O, 4mmol Zr(NO3)4·5H2O, 4mmol Ga(NO3)3·xH2O, 27.5mmol Cu(NO3)2·3H2O to make 100mL metal salt solution; weigh 60mmol Na2CO3 to make 120mL aqueous solution and place it in a 500mL four-necked beaker; insert a pH meter and a thermometer, drop the metal salt solution into the Na2CO3 aqueous solution at 70°C, and drop it in the reverse direction to cause a precipitation reaction. Calcination was carried out at 350°C in air for 4h. The other steps were the same as in Example 1. The detailed results are shown in Table 1.
[0071] Example 6
[0072] Weigh 12mmol Zn(NO3)2·6H2O, 4mmol Zr(NO3)4·5H2O, 4mmol Ga(NO3)3·xH2O, and 30mmol Cu(NO3)2·3H2O to make 100mL metal salt solution; weigh 60mmol Na2CO3 to make 120mL aqueous solution and place it in a 500mL four-necked beaker; insert a pH meter and a thermometer, drop the metal salt solution into the Na2CO3 aqueous solution at 70°C, and drop it in the reverse direction to cause a precipitation reaction. Calcination was carried out at 350°C in air for 4h. The other steps were the same as in Example 1. The detailed results are shown in Table 1.
[0073] Example 7
[0074] Weigh 9.5mmol Zn(NO3)2·6H2O, 4mmol Zr(NO3)4·5H2O, 4mmol Ga(NO3)3·xH2O, and 32.5mmol Cu(NO3)2·3H2O to make 100mL of metal salt solution; weigh 60mmol Na2CO3 to make 120mL of aqueous solution and place it in a 500mL four-necked beaker; insert a pH meter and a thermometer, drop the metal salt solution into the Na2CO3 aqueous solution at 70°C, and drop it in the reverse direction to cause a precipitation reaction. Calcination was carried out at 350°C in air for 4h. The other steps were the same as in Example 1. The detailed results are shown in Table 1.
[0075] Example 8
[0076] Weigh 14.5mmol Zn(NO3)2·6H2O, 4mmol Zr(NO3)4·5H2O, 4mmol Al(NO3)3·9H2O, 27.5mmol Cu(NO3)2·3H2O to make 100mL metal salt solution; weigh 60mmol Na2CO3 to make 120mL aqueous solution and place it in a 500mL four-necked beaker; insert a pH meter and a thermometer, drop the metal salt solution into the Na2CO3 aqueous solution at 70°C, and drop it in the reverse direction to cause a precipitation reaction. Calcination was carried out at 350°C in air for 4h. The other steps were the same as in Example 1. The detailed results are shown in Table 1.
[0077] Example 9
[0078] Weigh 12mmol Zn(NO3)2·6H2O, 4mmol Zr(NO3)4·5H2O, 4mmol Al(NO3)3·9H2O, 30mmol Cu(NO3)2·3H2O to make 100mL metal salt solution; weigh 60mmol Na2CO3 to make 120mL aqueous solution and place it in a 500mL four-necked beaker; insert a pH meter and a thermometer, drop the metal salt solution into the Na2CO3 aqueous solution at 70°C, and drop it in the reverse direction to cause a precipitation reaction. Calcination was carried out at 350°C in air for 4h. The other steps were the same as in Example 1. The detailed results are shown in Table 1.
[0079] Example 10
[0080] Weigh 9.5mmol Zn(NO3)2·6H2O, 4mmol Zr(NO3)4·5H2O, 4mmol Al(NO3)3·9H2O, 32.5mmol Cu(NO3)2·3H2O to make 100mL metal salt solution; weigh 60mmol Na2CO3 to make 120mL aqueous solution and place it in a 500mL four-necked beaker; insert a pH meter and a thermometer, drop the metal salt solution into the Na2CO3 aqueous solution at 70°C, and drop it in the reverse direction to cause a precipitation reaction. Calcination was carried out at 350°C in air for 4h. The other steps were the same as in Example 1. The detailed results are shown in Table 1.
[0081] Embodiment 11
[0082] Weigh 14.5mmol Zn(NO3)2·6H2O, 4mmol Zr(NO3)4·5H2O, 4mmol In(NO3)3·xH2O, and 27.5mmol Cu(NO3)2·3H2O to make 100mL metal salt solution; weigh 60mmol Na2CO3 to make 120mL aqueous solution and place it in a 500mL four-necked beaker; insert a pH meter and a thermometer, drop the metal salt solution into the Na2CO3 aqueous solution at 70°C, and drop it in the reverse direction to cause a precipitation reaction. Calcination was carried out at 350°C in air for 4h. The other steps were the same as in Example 1. The detailed results are shown in Table 1.
[0083] Example 12
[0084] Weigh 12mmol Zn(NO3)2·6H2O, 4mmol Zr(NO3)4·5H2O, 4mmol In(NO3)3·xH2O, and 30mmol Cu(NO3)2·3H2O to make 100mL metal salt solution; weigh 60mmol Na2CO3 to make 120mL aqueous solution and place it in a 500mL four-necked beaker; insert a pH meter and a thermometer, drop the metal salt solution into the Na2CO3 aqueous solution at 70°C, and drop it in the reverse direction to cause a precipitation reaction. Calcination was carried out at 350°C in air for 4h. The other steps were the same as in Example 1. The detailed results are shown in Table 1.
[0085] Embodiment 13
[0086] Weigh 9.5mmol Zn(NO3)2·6H2O, 4mmol Zr(NO3)4·5H2O, 4mmol In(NO3)3·xH2O, and 32.5mmol Cu(NO3)2·3H2O to make 100mL of metal salt solution; weigh 60mmol Na2CO3 to make 120mL of aqueous solution and place it in a 500mL four-necked beaker; insert a pH meter and a thermometer, drop the metal salt solution into the Na2CO3 aqueous solution at 70°C, and drop it in the reverse direction to cause a precipitation reaction. Calcination was carried out at 350°C in air for 4h. The other steps were the same as in Example 1. The detailed results are shown in Table 1.
[0087] Table 1 Catalytic performance evaluation results of the examples
[0088]
[0089] Wherein, in embodiment a: 0.5-10.0%, in embodiment b-c: 1.0-15%, in embodiment n, m, p: 35-65%, and x is a value that makes the catalyst electrically neutral.
[0090] Table 2 Microstructure data of catalysts with better catalytic performance in Example
[0091]
[0092]
[0093] The liquid sunlight zero-carbon emission methanol synthesis catalyst described in this application has uniformly dispersed active components, high catalyst strength, and can efficiently realize the co-hydrogenation of CO and CO2 into methanol, with few by-products and good stability. This series of catalysts is simple to prepare and suitable for large-scale preparation. It can be used to couple renewable energy hydrogen production with coal chemical industry and other chemical industries to synthesize liquid sunlight methanol and achieve zero-carbon emission methanol synthesis.
[0094] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. Application of a catalyst in zero-carbon emission methanol synthesis, characterized in that: The catalyst comprises an oxide solid solution; The oxides include zinc oxide, zirconium oxide, oxides of element X and oxides of element Y; The element X oxide is selected from copper oxide or palladium oxide; The oxide of the element Y is selected from the oxides of metal elements of Group IIIA, such as aluminum oxide, gallium oxide or indium oxide; The ratio of the sum of the molar amount of zinc in the zinc oxide and the molar amount of zirconium in the zirconium oxide to the sum of the molar amount of element X in the oxide of element X and the molar amount of element Y in the oxide of element Y is 1:6 to 6:1; The ratio of the molar amount of element X in the oxide of element X to the molar amount of element Y in the oxide of element Y is 1:7 to 7:1; The preparation method of the catalyst is a reverse precipitation method with a controlled end point pH value, wherein the end point pH value is 6 to 8; The method for preparing the catalyst comprises at least the following steps: Step (1): mixing raw materials containing a zinc source, a zirconium source, an element X source and an element Y source with deionized water and stirring to obtain a metal salt mixed solution; Step (2): adding a precipitant to deionized water and mixing and stirring to dissolve to obtain a precipitant solution; Step (3): adding the metal salt mixed solution obtained in step (1) to the precipitant solution obtained in step (2) at a certain temperature and stirring rate to cause a precipitation reaction, controlling the endpoint pH value of the precipitation solution and aging, washing, drying, and roasting to obtain the catalyst for synthesizing methanol; When the element X is copper, the source of the element X is selected from at least one of copper nitrate or acetate; When the element X is palladium, the source of the element X is selected from at least one of palladium nitrate or palladium chloride; When the element Y is gallium or indium, the source of the element Y is selected from nitrates; When the element Y is aluminum, the source of the element Y is selected from at least one of aluminum nitrate or aluminum acetate; When the catalyst is used for methanol synthesis, the composition of the raw synthesis gas is n(H2):n(CO2):n(CO):n(Ar)=67:8.2:21.2:
4.
2. The use according to claim 1, characterized in that: The sum of the molar amount of element X in the oxide of element X and the molar amount of element Y in the oxide of element Y accounts for 40-60% of the sum of the molar amount of zinc in zinc oxide and the molar amount of zirconium in zirconium oxide.
3. The use according to claim 1, characterized in that: The molar content relationship of the zinc source, zirconium source, element X source and element Y source: (Zn+Zr) / (X(X=Cu, Pd)+Y (Y=Al, Ga, In)) is 1:2~2:
1.
4. The use according to claim 1, characterized in that: In step (1), the zinc source is selected from at least one of zinc nitrate or zinc acetate; The zirconium source is selected from at least one of zirconium nitrate or zirconium oxynitrate; In the mixed solution, the total concentration of the zinc source, the zirconium source, the element X source and the element Y source is 0.3-0.8 mol / L.
5. The use according to claim 1, characterized in that: In step (2), the precipitant is selected from at least one of sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, sodium hydroxide or potassium hydroxide; The concentration of the precipitant in the precipitant solution is 0.3-0.8 mol / L; The molar ratio of the metal salt mixed solution to the precipitant solution obtained in step (2) is 1:1 to 1:1.2; The reverse drop precipitation for controlling the endpoint pH value is to drop the metal salt mixed solution into the precipitant solution for reaction; The dropping speed is 5-10 mL / min; The pH at the end point of the dropwise addition is 6-8.
6. The use according to claim 1, characterized in that: The temperature of the precipitation reaction is 50-80°C; The aging time after the precipitation reaction is 2 to 8 hours; The calcination temperature is 350-450°C; The calcination time is 3 to 8 hours; The method is also dried before roasting; The drying temperature is 60-120°C; The drying time is 6 to 15 hours.
7. The use according to claim 1, characterized in that: The synthesis of methanol comprises at least the following steps: The catalyst is loaded into a fixed bed reactor, and the raw synthesis gas is introduced. Under certain reaction conditions, the raw synthesis gas contacts the catalyst to undergo a catalytic reaction to obtain a product containing methanol.
8. The use according to claim 7, characterized in that: The catalyst is pre-treated; The pre-treatment process at least comprises the following steps: In an activation atmosphere, treat at 200-300°C for 2-24 hours; The pressure of the activation atmosphere is 0.1~1MPa; The activation atmosphere is selected from a mixed gas of hydrogen and an inert gas; The inert gas is selected from at least one of helium, argon or nitrogen; The volume concentration of hydrogen in the activation atmosphere is 5-99.999%.
9. The use according to claim 7, characterized in that: The pressure of the raw synthesis gas is 2-10 MPa; The feed space velocity of the raw synthesis gas is 4000~20000h –1 ; The temperature of the catalytic reaction is 180-280°C.