A high entropy phosphate catalyst and preparation method thereof

By developing the high-entropy phosphate catalyst NH4 (CoαNiβCuγZnδMnλ)PO4·H2O, the problem of low efficiency and easy deactivation of existing catalysts in catalyzing the hydrolysis of sodium borohydride has been solved, and the function of efficiently catalyzing the hydrolysis of sodium borohydride to produce hydrogen has been achieved. With long life and high conversion rate.

CN116328800BActive Publication Date: 2024-10-29LUOYANG ZHENGLIAN ENVIRONMENTAL TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310323163.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-29
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Existing catalysts have low efficiency and are easily deactivated in catalyzing the hydrolysis reaction of sodium borohydride, which limits the effective production of hydrogen, especially the low efficiency and short life of monometallic and bimetallic phosphate catalysts.

Method used

Develop a high-entropy phosphate catalyst NH4 (CoαNiβCuγZnδMnλ)PO4·H2O. By dissolving metal salts and reacting with phosphorus sources under hydrothermal conditions, urea is used to assist precipitation and adjust the pH value to form a high-entropy phosphate catalyst with high catalytic activity. .

Benefits of technology

The efficiency of the catalytic sodium borohydride hydrolysis reaction and the service life of the catalyst are improved. It has high thermodynamic and chemical stability. The catalyst raw materials are abundant, non-toxic, low in price, high in raw material conversion rate, simple in preparation process and high in production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116328800B_ABST
    Figure CN116328800B_ABST
Patent Text Reader

Abstract

The invention discloses a high entropy phosphate catalyst and a preparation method thereof. The catalyst mainly comprises NH4(Co α Ni β Cu γ Zn δ Mn λ )PO4·H2O, wherein α+β+γ+δ+λ=1, 0.05<α, β, γ, δ, λ<0.35. The preparation method comprises the following steps: adding a phosphorus source and urea to an aqueous solution of a cobalt salt, a nickel salt, a copper salt, a zinc salt and a manganese salt, stirring until completely dissolved, transferring to a reactor for a hydrothermal reaction, washing and drying to obtain a product. The catalyst raw material disclosed in the present invention has abundant sources, is non-toxic, has a low price, a simple preparation process and high production efficiency. The present invention obtains a high entropy phosphate catalyst by a one-step hydrothermal method, does not require complex processes such as calcination, and has a high raw material conversion rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of inorganic functional materials, and specifically relates to a high entropy catalyst and a preparation method thereof. Background Art

[0002] As an efficient, clean, sustainable and "carbon-free" energy, hydrogen energy has received widespread attention from countries around the world and is hailed as the energy of the 21st century. Developing a hydrogen energy economy is a permanent strategic choice for mankind to get rid of its dependence on fossil energy and ensure energy security. However, hydrogen energy is subject to many restrictions in practical applications. One of the most important technical challenges is the storage, transportation and effective release of hydrogen. Among various chemical hydrogen storage materials, sodium borohydride can be hydrolyzed in the presence of a catalyst to produce the following reaction: NaBH4+2H2O=NaBO2+4H2↑, and 1 mole of sodium borohydride can produce 4 moles of hydrogen.

[0003] However, the hydrolysis reaction of sodium borohydride itself is extremely slow, and the hydrolysis rate is extremely low, which greatly limits the development of sodium borohydride hydrolysis hydrogen production technology. Studies have shown that the hydrolysis reaction of sodium borohydride can be greatly accelerated under the action of a suitable catalyst. Metal catalysts have been widely studied because of their high catalytic activity. Among them, precious metals are expensive, which limits their use, while non-precious metals are low in price and high in reserves. In addition, in recent years, studies have found that the catalytic activity of some non-precious metal catalysts has been significantly improved.

[0004] Among various cheap transition metal catalysts, phosphate catalysts show certain activity in catalyzing hydrogen production from sodium borohydride. However, monometallic and bimetallic low entropy phosphate catalysts have the disadvantages of low efficiency and easy deactivation. Therefore, high entropy compounds with multiple catalytic active sites have received extensive attention. Compared with monometallic and bimetallic component catalysts, multimetallic high entropy catalysts have better application prospects in catalytic reactions, because the active metals can not only provide new active sites, but also promote the interaction of multiple metal components to improve the performance of catalytic hydrogen production from sodium borohydride. However, there is currently no relevant report on the synthesis of high entropy phosphate catalysts and their application in catalytic hydrolysis of sodium borohydride to produce hydrogen. The purpose of the present invention is to develop a high entropy phosphate catalyst for catalytic hydrolysis of sodium borohydride to produce hydrogen. Summary of the invention

[0005] In order to overcome the above-mentioned deficiencies in the prior art, the object of the present invention is to develop a high entropy phosphate catalyst for catalyzing the hydrolysis of sodium borohydride to produce hydrogen.

[0006] A high entropy phosphate catalyst, the catalyst mainly composed of NH4(Co α Ni β Cu γ Zn δ Mnλ )PO4·H2O, where α+β+γ+δ+λ=1, 0.05<α, β, γ, δ, λ<0.35.

[0007] This patent also discloses a preparation method for the above-mentioned high entropy phosphate catalyst, comprising the following steps: step 1, dissolving cobalt salt, nickel salt, copper salt, zinc salt, and manganese salt in water to prepare a mixed solution; step 2, adding a certain amount of urea and phosphorus source to the mixed solution described in step 1 under stirring, transferring them to a reactor after complete dissolution, reacting for a certain time under a certain temperature, washing the reaction product with deionized water and ethanol, and drying to obtain a high entropy phosphate catalyst.

[0008] Preferably, the cobalt salt concentration in step 1 is 0.05-5 mol / L, the nickel salt concentration is 0.05-5 mol / L, the copper salt concentration is 0.05-5 mol / L, the zinc salt concentration is 0.05-5 mol / L, and the manganese salt concentration is 0.05-5 mol / L; the cobalt salt, nickel salt, copper salt, zinc salt, and manganese salt can be one or more of chlorides, nitrates, sulfates, or acetates.

[0009] Preferably, the molar ratio of the cobalt salt, nickel salt, copper salt, zinc salt and manganese salt in step 1 is α:β:γ:δ:λ (1-4):(1-4):(1-4):(1-4).

[0010] Preferably, the molar ratio of the cobalt salt to urea in step 2 is 1:20 to 1:280, and the molar ratio of the cobalt salt to the phosphorus source is 1:0.5 to 1:10.

[0011] Preferably, in step 2, the phosphorus source is one or more of ammonium dihydrogen phosphate, sodium dihydrogen phosphate, potassium dihydrogen phosphate, disodium hydrogen phosphate, diammonium hydrogen phosphate, dipotassium hydrogen phosphate, ammonium phosphate, sodium phosphate, potassium phosphate and phosphoric acid.

[0012] Preferably, the reaction temperature in step 2 is 130-180° C., and the reaction time is 4-48 hours.

[0013] Preferably, the drying temperature in step 2 is 30 to 90° C. and the drying time is 6 to 48 hours.

[0014] The above technical scheme has the following beneficial effects: the high entropy phosphate catalyst in the present invention has high thermodynamic and chemical stability, has a long service life as a catalyst for sodium borohydride hydrolysis, and has excellent catalytic sodium borohydride hydrolysis hydrogen production function. The catalyst raw material source is abundant, non-toxic, low in price, and has a high raw material conversion rate. During the preparation process, the phosphorus source plays the role of the main precipitant in the reaction process, and the phosphorus source must be added to form phosphate. Since the precipitation ability of the phosphorus source itself is insufficient, urea plays the role of auxiliary precipitation and pH adjustment. During the heating process, urea will first decompose to produce ammonia and carbon dioxide, and further generate hydroxide ions under hydrothermal conditions. In the supersaturated solution, the hydroxide ions and metal ions are combined to form small crystal nuclei, which is conducive to the growth of phosphate crystals. The hydroxide ions will eventually be replaced by phosphate. The preparation method is simple in process and high in production efficiency. The product is obtained by one hydrothermal step, and no other complicated steps are required, which is convenient for preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 is a scanning electron microscope photograph of the high entropy phosphate catalyst prepared in Example 1 of the present invention;

[0016] Figure 2 is the XRD diagram of the high entropy phosphate catalyst prepared in Example 1 of the present invention;

[0017] Figure 3 This is a performance diagram of the high entropy phosphate catalyst prepared in Example 1 of the present invention catalyzing the hydrolysis of sodium borohydride to produce hydrogen. DETAILED DESCRIPTION

[0018] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.

[0019] The example embodiments will now be described more fully with reference to the accompanying drawings. However, the example embodiments can be implemented in a variety of forms and should not be construed as being limited to the examples set forth herein; on the contrary, these embodiments are provided so that the present invention will be more comprehensive and complete, and the concept of the example embodiments will be fully conveyed to those skilled in the art. The described features, structures, or characteristics may be combined in one or more embodiments in any suitable manner. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present invention. However, those skilled in the art will appreciate that the technical solutions of the present invention may be practiced while omitting one or more of the specific details, or other methods, components, devices, steps, etc. may be adopted. In other cases, the known technical solutions are not shown or described in detail to avoid obscuring the various aspects of the present invention. The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute an improper limitation of the present invention.

[0020] This patent discloses a high entropy phosphate catalyst, which is mainly composed of NH4(Co α Ni β Cu γ Zn δ Mn λ )PO4·H2O, where a+β+γ+δ+λ=1, 0.05<α, β, γ, δ, λ<0.35.

[0021] This patent also discloses a method for preparing the above-mentioned high entropy phosphate catalyst. The preparation method of this patent is further described below with a specific example:

[0022] A preparation method of a high entropy phosphate catalyst comprises the following steps: dissolving 0.4 mmol of cobalt chloride, nickel chloride, copper chloride, zinc chloride and manganese chloride in 80 ml of deionized water to prepare a mixed solution, then adding 1.3 mmol of ammonium dihydrogen phosphate and 56 mmol of urea under stirring conditions, transferring the solution to a reaction kettle after complete dissolution, reacting at 150° C. for 6 hours, washing the precipitate with deionized water for 2 to 3 times, then washing the precipitate with ethanol for 2 to 3 times, and finally drying at 80° C. for 12 hours to obtain the high entropy phosphate catalyst.

[0023] The morphology of the high entropy phosphate catalyst prepared by the above preparation method is as follows: Figure 1 As shown in Figure 2, it can be seen that the high entropy phosphate catalyst has a two-dimensional sheet morphology. Figure 2As shown, the XRD diffraction peak position of the product is consistent with the peak position of the standard card PDF#50-1559, indicating that the product has the same crystal structure as the substance corresponding to the standard card PDF#50-05549. No other impurity peaks appear, indicating that the purity of the product is high.

[0024] The performance of the high entropy phosphate catalyst for catalyzing the hydrolysis of sodium borohydride is shown in the figure below. Figure 3 As shown, it can be seen that without adding a catalyst, the hydrogen production is only 1.75 mL after 100 minutes of reaction, while after adding the catalyst in Example 1, the hydrogen production increases to 82.6 mL, and the hydrogen production per unit mass reaches 737 mmol / g. This shows that the synthesized high entropy phosphate catalyst has excellent performance in catalyzing the hydrolysis of sodium borohydride to produce hydrogen.

[0025] The concentration of cobalt salt in the preparation method is 0.05-5 mol / L, the concentration of nickel salt is 0.05-5 mol / L, the concentration of copper salt is 0.05-5 mol / L, the concentration of zinc salt is 0.05-5 mol / L, and the concentration of manganese salt is 0.05-5 mol / L; the cobalt salt, nickel salt, copper salt, zinc salt, and manganese salt can be one or more of chloride, nitrate, sulfate, or acetate. The molar ratio of cobalt salt, nickel salt, copper salt, zinc salt, and manganese salt is α:β:γ:δ:λ, which is (1-4):(1-4):(1-4):(1-4):(1-4). During the preparation process, it can be adjusted according to actual needs.

[0026] The molar ratio of cobalt salt to urea can be controlled at 1:20-1:280, the molar ratio of cobalt salt to phosphorus source is 1:0.5-1:10, and the phosphorus source is one or more of diammonium phosphate, sodium dihydrogen phosphate, potassium dihydrogen phosphate, disodium hydrogen phosphate, diammonium hydrogen phosphate, dipotassium hydrogen phosphate, ammonium phosphate, sodium phosphate, potassium phosphate and phosphoric acid.

[0027] The reaction temperature in the reactor can be adjusted within the range of 130 to 180° C., the reaction time is 4 to 48 hours, the drying temperature can be adjusted within the range of 30 to 90° C., and the drying time is 6 to 48 hours.

[0028] In the preparation process of the preparation method, the phosphorus source plays the role of the main precipitant in the reaction process, and the phosphorus source must be added to form phosphate. Since the precipitation capacity of the phosphorus source itself is insufficient, urea plays the role of auxiliary precipitation and pH adjustment. During the heating process, urea will first decompose to produce ammonia and carbon dioxide, and further generate hydroxide ions under hydrothermal conditions. In the supersaturated solution, the hydroxide ions and metal ions combine to form small crystal nuclei, which is conducive to the growth of phosphate crystals. The hydroxide ions will eventually be replaced by phosphate. The preparation method has a simple process and high production efficiency. The product is obtained by one hydrothermal step, and no other complex steps are required, which is easy to prepare. The catalyst raw material source is abundant, non-toxic, low in price, and high in raw material conversion rate. The prepared high-entropy phosphate catalyst has high thermodynamic and chemical stability, has a long service life as a catalyst for the hydrolysis of sodium borohydride, and has excellent catalytic sodium borohydride hydrolysis hydrogen production function.

[0029] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A high entropy phosphate catalyst, characterized in that: The catalyst composition is NH4(Co α Ni β Cu γ Zn δ Mn λ )PO4·H2O, wherein α+β+γ+δ+λ=1, 0.05<α, β, γ, δ, λ<0.

35. The preparation method of the catalyst comprises the following steps: 1) dissolving cobalt salt, nickel salt, copper salt, zinc salt and manganese salt in water to prepare a mixed solution; 2) adding a certain amount of urea and phosphorus source to the mixed solution described in step 1) under stirring, transferring them to a reactor after they are completely dissolved, the reaction temperature is 130-180°C, the reaction time is 4-48 hours, washing the reaction product with deionized water and ethanol, and drying to obtain a high entropy phosphate catalyst.

2. A method for preparing the high entropy phosphate catalyst according to claim 1, characterized in that: The following steps are involved: Step 1, dissolving cobalt salt, nickel salt, copper salt, zinc salt and manganese salt in water to prepare a mixed solution; Step 2: add a certain amount of urea and phosphorus source to the mixed solution described in step 1 under stirring, transfer to a reactor after complete dissolution, the reaction temperature is 130-180° C., the reaction time is 4-48 hours, wash the reaction product with deionized water and ethanol, and dry to obtain a high entropy phosphate catalyst.

3. The preparation method according to claim 2, characterized in that: The cobalt salt concentration in step 1 is 0.05-5 mol / L, the nickel salt concentration is 0.05-5 mol / L, the copper salt concentration is 0.05-5 mol / L, the zinc salt concentration is 0.05-5 mol / L, and the manganese salt concentration is 0.05-5 mol / L; the cobalt salt, nickel salt, copper salt, zinc salt, and manganese salt are one or more of chlorides, nitrates, sulfates, or acetates.

4. The preparation method according to claim 2, characterized in that: The molar ratio of the cobalt salt, nickel salt, copper salt, zinc salt and manganese salt in step 1 is (1-4):(1-4):(1-4):(1-4):(1-4).

5. The preparation method according to claim 2, characterized in that: The molar ratio of the cobalt salt to urea in step 2 is 1:20 to 1:280, and the molar ratio of the cobalt salt to the phosphorus source is 1:0.5 to 1:

10.

6. The preparation method according to claim 2, characterized in that: In the step 2, the phosphorus source is one or more of ammonium dihydrogen phosphate, sodium dihydrogen phosphate, potassium dihydrogen phosphate, disodium hydrogen phosphate, diammonium hydrogen phosphate, dipotassium hydrogen phosphate, ammonium phosphate, sodium phosphate, potassium phosphate and phosphoric acid.

7. The preparation method according to claim 2, characterized in that: The drying temperature in step 2 is 30 to 90° C. and the drying time is 6 to 48 hours.

Citation Information

Patent Citations

  • One-step preparation method and application of nano transition metal phosphates

    CN105645371A

  • Preparation method of cobalt copper phosphate microspheres, and application of cobalt copper phosphate microspheres in catalyzing hydrolysis of ammonia borane to produce hydrogen

    CN110835103A