Composite high-strength concrete and preparation process
By using modified glass fiber and aramid fiber in concrete, combined with cationic chloroprene latex and EVA emulsion, the problem of insufficient strength and crack resistance of glass fiber reinforced concrete is solved, and the improvement of high strength and crack resistance is achieved.
Patent Information
- Application Number
- CN202310299707.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-03-25
AI Technical Summary
Existing glass fiber reinforced concrete has shortcomings in terms of strength and crack resistance. Too little glass fiber can not improve the strength, while too much will lead to cracking.
Acrylic grafted glass fiber and dopamine grafted aramid fiber, combined with cationic chloroprene emulsion and EVA emulsion, reduce the stress concentration between fibers through modification treatment, improve the strength and crack resistance of concrete, and pass fly ash and slag. , the combination of mineral powder and silicon powder improves the compactness and bondability of concrete.
The compressive strength and tensile strength of concrete are significantly improved, cracking phenomenon caused by stress concentration is reduced, and the overall strength and crack resistance of concrete are enhanced.
Smart Images

Figure BDA0004144622730000041 
Figure BDA0004144622730000061 
Figure BDA0004144622730000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of concrete preparation, and in particular relates to a composite high-strength concrete and a preparation process thereof. Background Art
[0002] Concrete is a multiphase composite material formed by bonding sand and gravel aggregates with cementitious materials. Concrete plays an important role in building materials. Among them, since high-strength concrete is much stronger than ordinary concrete and has much smaller deformation under the same stress conditions, its structural bearing capacity is significantly improved. Therefore, high-strength concrete has more applications in large-scale special and important projects. For the use of concrete in large stadium stands, circular column structures and other parts, due to frequent use and dense crowds, the strength requirements for concrete are more stringent.
[0003] Glass fiber reinforced concrete (GRC for short) is a cement-based composite material formed by embedding alkali-resistant glass fibers into cement-based materials. Glass fibers have high tensile strength and elastic modulus, and can improve the tensile strength of cement-based composite materials. However, too little glass fiber addition will not play a role in strengthening the strength, while too much glass fiber addition will cause concrete cracking due to stress concentration.
[0004] Therefore, the present application is in urgent need of developing a high-strength and crack-resistant concrete. Summary of the invention
[0005] In order to improve the strength and crack resistance of concrete, the present application provides a composite high-strength concrete and a preparation process.
[0006] In a first aspect, the present application provides a composite high-strength concrete, which is implemented by the following technical solution:
[0007] A composite high-strength concrete comprises, by weight, 300-400 parts of cement, 20-30 parts of coarse aggregate, 120-160 parts of fine aggregate, 60-80 parts of fly ash, 60-80 parts of slag, 20-30 parts of mineral powder, 30-40 parts of silicon powder, 30-40 parts of acrylic acid-grafted glass fiber, 40-50 parts of dopamine-grafted aramid fiber, 1-1.5 parts of calcium lignin sulfonate, 10-20 parts of cationic chloroprene rubber latex, 20-30 parts of EVA latex and 120-200 parts of water.
[0008] By adopting the above technical scheme, fly ash has a certain volcanic ash activity, which can generate hydrated calcium silicate to improve the strength and impermeability of concrete; slag and mineral powder can effectively improve the density of concrete and improve the strength of concrete; the fineness of silica powder is relatively fine, which can effectively fill the gaps of cement and improve the density of concrete. The addition of acrylic acid grafted glass fiber and dopamine grafted aramid fiber significantly improves the strength of concrete, while reducing the agglomeration phenomenon between fibers, thereby reducing the cracking phenomenon caused by stress concentration. The cationic chloroprene latex emulsion and EVA emulsion work together, not only improving the bonding between the various raw materials of concrete preparation and improving the strength of concrete, but also interweaving with acrylic acid grafted glass fiber and dopamine grafted aramid fiber into a network, further dispersing the stress of acrylic acid grafted glass fiber and dopamine grafted aramid fiber, while making fly ash, mineral powder and silica powder more dense, thereby improving the crack resistance and strength of concrete. Calcium lignin sulfonate is used as a water reducer in concrete. After being added to concrete, it is beneficial to reduce the porosity of concrete, thereby helping to improve the strength of concrete.
[0009] Preferably, the method for preparing the acrylic acid grafted glass fiber comprises the following steps:
[0010] The glass fiber, acrylic acid and silane coupling agent are mixed in a mass ratio of 1:(0.2-0.3):(0.1-0.15), reacted at 80-90°C for 6-8h, washed, filtered and dried to obtain acrylic acid grafted glass fiber.
[0011] By adopting the above technical scheme, the acrylic grafted glass fiber prepared by modifying acrylic acid and silane coupling agent improves the adhesion between the glass fiber and the other raw materials, significantly reduces the stress concentration of the glass fiber, significantly improves the splitting tensile strength of the concrete, and also improves the compressive strength to a certain extent.
[0012] Preferably, the acrylic acid is an aqueous hydroxy acrylic acid dispersion.
[0013] By adopting the above technical solution, the water-based hydroxy acrylic dispersion has a high hydroxy content, which is more conducive to reducing the stress concentration of glass fibers, thereby improving the splitting tensile strength of concrete.
[0014] Preferably, the silane coupling agent is prepared by mixing (N-anilino)methyltriethoxysilane and diethylaminomethyltriethoxysilane in a mass ratio of 1:(1.6-2).
[0015] The silane coupling agent compounded with (N-anilino)methyltriethoxysilane and diethylaminomethyltriethoxysilane has higher cross-linking activity for glass fibers. In addition, (N-anilino)methyltriethoxysilane contains a rigid benzene ring, which has conjugation and hydrogen bonding effects with dopamine-grafted aramid fibers, further reducing the stress concentration of glass fibers and aramid fibers and improving the splitting tensile strength of concrete.
[0016] Preferably, the method for preparing the dopamine grafted aramid fiber comprises the following steps:
[0017] The aramid fiber is immersed in acetone, washed, dried, immersed in potassium permanganate solution, washed, dried, and immersed in dopamine mixed solution, washed, and dried to obtain dopamine-grafted aramid fiber; the dopamine mixed solution contains diethylenetriaminepropyltrimethoxysilane and dopamine hydrochloride.
[0018] By adopting the above technical scheme, the aramid fiber is washed with acetone and then treated with potassium permanganate to improve the reactivity of the aramid fiber. Then, the aramid fiber is reacted with dopamine and diethylenetriaminopropyltrimethoxysilane to significantly reduce the agglomeration of the aramid fiber, and cracking due to stress concentration almost does not occur. Diethylenetriaminopropyltrimethoxysilane is triaminosilane and has hydrogen bonding with dopamine, which improves the wettability of the aramid fiber and the interfacial adhesion between the aramid fiber and other preparation raw materials, thereby improving the compressive strength and splitting tensile strength of the concrete.
[0019] Preferably, the concentration of dopamine hydrochloride in the dopamine mixed solution is 20-30 g / L.
[0020] By adopting the above technical solution, the present application controls the concentration of dopamine hydrochloride to 20-30 g / L, thereby improving the wettability of the aramid fiber.
[0021] Preferably, the concentration of diethylenetriaminopropyltrimethoxysilane in the dopamine mixed solution is 7-10 g / L.
[0022] By adopting the above technical solution, the present application controls the concentration of diethylenetriaminopropyltrimethoxysilane to 7-10 g / L, thereby improving the adhesion between the aramid fiber and the other preparation raw materials.
[0023] In a second aspect, the present application provides a process for preparing composite high-strength concrete, which is implemented by the following technical solution: A process for preparing composite high-strength concrete, comprising the following steps:
[0024] S1. Screening coarse aggregate and fine aggregate to obtain aggregate;
[0025] S2, mixing and crushing fly ash, slag, mineral powder and silicon powder to obtain crushed material;
[0026] S3. Mix cement, aggregate, crushed material, acrylic acid grafted glass fiber, dopamine grafted aramid fiber, calcium lignin sulfonate, cationic chloroprene rubber latex, EVA emulsion and water to obtain composite high-strength concrete.
[0027] By adopting the above technical solution, the particle size of coarse aggregate and fine aggregate can be screened, which can reduce the influence of different aggregate diameters on the strength of concrete to a certain extent. Crushing fly ash, slag, mineral powder and silica powder can improve the density of concrete, thereby improving the strength of concrete.
[0028] Preferably, the particle size of the coarse aggregate is 8-10 mm.
[0029] By adopting the above technical solution, the particle size of the coarse aggregate is controlled to 8-10mm in the present application, which can reduce the stress concentration at the interface between the aggregate and the hardened cement paste, increase the interface area between the hardened cement paste and the coarse aggregate, make the concrete bear the force evenly when bearing the load, and improve the strength of the concrete.
[0030] In summary, this application has the following beneficial effects:
[0031] 1. The present application adopts acrylic acid grafted glass fiber and dopamine grafted aramid fiber to improve the strength of concrete and reduce the agglomeration phenomenon between fibers, thereby reducing the cracking phenomenon caused by stress concentration.
[0032] 2. This application adopts cationic chloroprene rubber latex emulsion and EVA emulsion to improve the adhesion between the various raw materials used in the preparation of concrete, and improve the crack resistance and strength of concrete.
[0033] 3. The present application adopts acrylic acid grafted glass fiber prepared by co-modification of acrylic acid and silane coupling agent, which reduces the stress concentration of glass fiber and improves the crack resistance and splitting tensile strength of concrete.
[0034] 4. This application uses water-based hydroxy acrylic dispersion to improve the splitting tensile strength of concrete.
[0035] 5. The present application adopts a silane coupling agent compounded with (N-anilino)methyltriethoxysilane and diethylaminomethyltriethoxysilane to improve the splitting tensile strength of concrete.
[0036] 6. The present application adopts dopamine and diethylenetriaminepropyltrimethoxysilane to modify the aramid fiber treated with potassium manganate, which reduces the agglomeration of the aramid fiber and improves the wettability of the aramid fiber, thereby improving the compressive strength and splitting tensile strength of the concrete. DETAILED DESCRIPTION
[0037] The present application is further described in detail below in conjunction with embodiments.
[0038] Preparation Example
[0039] Preparation Example 1-8 provides an acrylic grafted glass fiber, and Preparation Example 1 is used as an example for description below.
[0040] The acrylic acid grafted glass fiber provided in Preparation Example 1 is prepared in the following steps:
[0041] 10 kg of glass fiber, 2 kg of acrylic acid and 1 kg of 3-aminopropyltriethoxysilane were mixed and reacted at 80°C for 8 hours. After the reaction, they were added to anhydrous ethanol, stirred and washed, the filtrate was filtered out, washed three times with anhydrous ethanol, and dried at 80°C for 12 hours to obtain acrylic acid-grafted glass fiber.
[0042] The only difference between Preparation Example 2-3 and Preparation Example 1 is that the quality of the raw materials for preparing the acrylic grafted glass fiber is different, as shown in Table 1.
[0043] Table 1 Mass of each raw material for preparing acrylic acid grafted glass fiber in Preparation Example 1-3 / kg
[0044]
[0045] Preparation Example 4 is different from Preparation Example 3 only in that acrylic acid is replaced with an aqueous hydroxy acrylic dispersion (brand number QR642, purchased from Qingyuan Qingrun New Material Technology Co., Ltd.).
[0046] Preparation Example 5 is different from Preparation Example 4 only in that 3-aminopropyltriethoxysilane is replaced by (N-anilino)methyltriethoxysilane.
[0047] Preparation Example 6 is different from Preparation Example 4 only in that 3-aminopropyltriethoxysilane is replaced by diethylaminomethyltriethoxysilane.
[0048] Preparation Example 7 is different from Preparation Example 4 only in that the mass of 3-aminopropyltriethoxysilane is replaced by a mixture of (N-anilino)methyltriethoxysilane and diethylaminomethyltriethoxysilane, and the mass ratio of (N-anilino)methyltriethoxysilane to diethylaminomethyltriethoxysilane is 1:1.6.
[0049] Preparation Example 8 is different from Preparation Example 7 only in that the mass ratio of (N-anilino)methyltriethoxysilane to diethylaminomethyltriethoxysilane is 1:2.
[0050] Preparation Examples 9-11 provide a dopamine mixed solution, and Preparation Example 9 is used as an example for description below.
[0051] The dopamine mixed solution provided in Preparation Example 9 is prepared in the following steps:
[0052] 200 g of dopamine hydrochloride and 70 g of diethylenetriaminopropyltrimethoxysilane were added to 10 L of Tris-HCl buffer solution with a pH of 8.5, and the mixture was stirred evenly to obtain a dopamine mixed solution.
[0053] Preparation Example 10 is different from Preparation Example 9 in that the mass of dopamine hydrochloride is 300 g.
[0054] Preparation Example 11 is different from Preparation Example 10 in that the mass of diethylenetriaminopropyltrimethoxysilane is 100 g.
[0055] Preparation Examples 12-14 provide a dopamine grafted aramid fiber, and Preparation Example 12 is used as an example for explanation below.
[0056] The dopamine-grafted aramid fiber provided in Preparation Example 12 is prepared in the following steps:
[0057] The aramid fiber is soaked in acetone for 12 hours, taken out and cleaned with ultrasonic waves for 1 hour, then washed with deionized water three times and ethanol three times, dried naturally at 25°C, soaked in 1 mol / L potassium permanganate solution for 3 hours, taken out and washed with deionized water until neutral, dried naturally at 25°C, soaked in dopamine mixed solution for 12 hours, taken out and washed with deionized water three times and ethanol three times, dried naturally at 25°C, to obtain dopamine-grafted aramid fiber;
[0058] Among them, the dopamine mixed solution comes from Preparation Example 9.
[0059] Preparation Example 13 is different from Preparation Example 12 in that the dopamine mixed solution is derived from Preparation Example 10.
[0060] Preparation Example 14 is different from Preparation Example 12 in that the dopamine mixed solution is derived from Preparation Example 11.
[0061] Preparation Comparative Example
[0062] Preparation Comparative Example 1-2 provides a dopamine mixed solution.
[0063] Comparative Example 1 was prepared, which differed from Preparation Example 9 only in that an equal amount of diethylenetriaminopropyltrimethoxysilane was replaced by 3-aminopropyltriethoxysilane.
[0064] Comparative Example 2 was prepared, which was different from Preparation Example 9 only in that no diethylenetriaminopropyltrimethoxysilane was added.
[0065] Preparation Comparative Example 3-4 provides a dopamine grafted aramid fiber.
[0066] Preparation Example 3 is different from Preparation Example 12 only in that the dopamine mixed solution is derived from Preparation Example 1.
[0067] Preparation Example 4 is different from Preparation Example 12 only in that the dopamine mixed solution is derived from Preparation Example 2.
[0068] The modified glass fiber provided in Comparative Example 5 is prepared by the following steps:
[0069] 10 kg of glass fiber and 1 kg of 3-aminopropyltriethoxysilane were mixed and reacted at 80°C for 8 hours. After the reaction, the mixture was added to anhydrous ethanol, stirred and washed, the filtrate was filtered out, washed three times with anhydrous ethanol, and dried at 80°C for 12 hours to obtain modified glass fiber.
[0070] Example
[0071] Embodiments 1-15 provide a composite high-strength concrete, which is described below using Embodiment 1 as an example.
[0072] The composite high-strength concrete provided in Example 1 is prepared in the following steps:
[0073] S1, screen out 2kg of gravel with a particle size of 8-10mm and 12kg of sand with a particle size of 0.25-0.5mm, and mix them to obtain aggregate;
[0074] S2, 6kg fly ash, 6kg slag, 2kg mineral powder and 3kg silicon powder are mixed and crushed to a particle size of less than 3mm to obtain a crushed material; S3, 30kg 42.5R grade silicate cement, the above aggregate, the above crushed material, 3kg acrylic acid grafted glass fiber, 4kg dopamine grafted aramid fiber, 0.1kg lignin sulfonate calcium, 1kg cationic chloroprene latex, 2kg EVA emulsion and 12kg water are mixed and stirred evenly to obtain a composite high-strength concrete;
[0075] Wherein, the acrylic acid grafted glass fiber is derived from Preparation Example 1;
[0076] Dopamine grafted aramid fiber is derived from Preparation Example 12;
[0077] Cationic chloroprene latex emulsion, brand name JBD07051, purchased from Shandong Jinbangde New Building Materials Co., Ltd.;
[0078] EVA emulsion, brand DA102H, was purchased from Nanjing Baiju Technology Co., Ltd.
[0079] The only difference between Example 2-4 and Example 1 is that the quality of the raw materials for preparing the composite high-strength concrete is different, as shown in Table 2.
[0080] Table 2 Mass of raw materials for preparing composite high-strength concrete in Examples 1-4 / kg
[0081]
[0082] The only difference between Examples 5-11 and Example 3 is that the sources of the acrylic-grafted glass fibers are different, as shown in Table 3.
[0083] Table 3 Sources of acrylic acid grafted glass fibers in Examples 3, 5-11
[0084] Group Example 3 Example 5 Example 6 Example 7 Acrylic Grafted Glass Fiber Source Preparation Example 1 Preparation Example 2 Preparation Example 3 Preparation Example 4 Group Example 8 Example 9 Example 10 Embodiment 11 Acrylic Grafted Glass Fiber Source Preparation Example 5 Preparation Example 6 Preparation Example 7 Preparation Example 8
[0085] Example 12 is different from Example 10 only in that the dopamine grafted aramid fiber is derived from Preparation Example 13.
[0086] Example 13 is different from Example 10 only in that the dopamine grafted aramid fiber is derived from Preparation Example 14.
[0087] Example 14 is different from Example 4 only in that the dopamine grafted aramid fiber is derived from Preparation Comparative Example 3.
[0088] Example 15 is different from Example 4 only in that the dopamine grafted aramid fiber is derived from Preparation Comparative Example 4.
[0089] Comparative Example
[0090] Comparative Example 1 is different from Example 15 only in that the dopamine-grafted aramid fiber is replaced with aramid fiber of equal mass.
[0091] Comparative Example 2 is different from Example 15 only in that the acrylic grafted glass fiber of equal mass is replaced by glass fiber.
[0092] Comparative Example 3 is different from Example 15 only in that the acrylic grafted glass fiber of equal mass is replaced by the modified glass fiber prepared in Comparative Example 5.
[0093] Comparative Example 4 is different from Example 15 only in that the cationic chloroprene rubber latex emulsion is replaced by EVA emulsion in equal mass.
[0094] Comparative Example 5 is different from Example 15 only in that the EVA emulsion of equal mass is replaced by cationic chloroprene latex emulsion.
[0095] Performance testing
[0096] The composite high-strength concrete prepared in Examples 1-15 and Comparative Examples 1-5 was used as a test sample (cubic standard specimen of 150 mm×150 mm×150 mm), and after standard curing for 28 days, the following performance tests were performed.
[0097] 1. Compressive strength: The compressive strength was tested in accordance with GB / T 50081-2002 “Standard for Test Methods for Mechanical Properties of Ordinary Concrete”. The test results are shown in Table 4.
[0098] 2. Split tensile strength: The split tensile strength was tested in accordance with GB / T 50081-2002 “Standard for Test Methods for Mechanical Properties of Ordinary Concrete”. The test results are shown in Table 4.
[0099] 3. Appearance: Observe whether there are cracks on the surface of each group of samples and record the length of the cracks. The test results are shown in Table 4.
[0100] Table 4 Test results
[0101]
[0102]
[0103] The following describes the present application in detail with respect to the test data in Table 4.
[0104] By comparing the data of Examples 1-15 and Comparative Examples 1-5, it was found that the composite high-strength concrete prepared in Examples 1-15 had no cracks after 28 days of curing, while each group in Comparative Examples 1-5 had cracks of varying degrees, and the compressive strength and splitting tensile strength of the composite high-strength concrete in Comparative Examples 1-5 were lower than those in Examples 1-15, indicating that the composite high-strength concrete prepared in the present application has high strength and good crack resistance.
[0105] By comparing Example 15 with Comparative Examples 1 and 3, it is found that replacing glass fiber with acrylic grafted glass fiber is beneficial to improving the crack resistance of concrete, and the compressive strength and splitting tensile strength of concrete are slightly improved.
[0106] By comparing Example 15 with Comparative Example 2, it is found that dopamine-grafted aramid fiber replaces aramid fiber, which improves the crack resistance of concrete and improves the compatibility of aramid fiber with other components without damaging the mechanical properties of aramid fiber, thereby improving the strength of concrete to a certain extent.
[0107] By comparing Example 15 with Comparative Examples 4 and 5, it is found that the cationic chloroprene rubber latex emulsion and the EVA emulsion work together to improve the crack resistance and strength of the concrete.
[0108] By comparing Example 4 with Examples 14-15, it is found that the aramid fiber modified with diethylenetriaminopropyltrimethoxysilane and dopamine hydrochloride has good wettability and high interface adhesion, thereby improving the compressive strength and splitting tensile strength of concrete.
[0109] By comparing Example 7 with Example 6, it is found that the acrylic grafted glass fiber prepared by using the aqueous hydroxy acrylic dispersion and the silane coupling agent in Example 7 improves the splitting tensile strength of the concrete.
[0110] By comparing Example 11 with Examples 7-10, it is found that the silane coupling agent compounded with (N-anilino)methyltriethoxysilane and diethylaminomethyltriethoxysilane reduces the stress concentration of glass fiber and aramid fiber and improves the splitting tensile strength of concrete.
[0111] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A composite high-strength concrete, characterized in that: The raw materials for preparation include 300-400 parts of cement, 20-30 parts of coarse aggregate, 120-160 parts of fine aggregate, 60-80 parts of fly ash, 60-80 parts of slag, 20-30 parts of mineral powder, 30-40 parts of silicon powder, 30-40 parts of acrylic acid grafted glass fiber, 40-50 parts of dopamine grafted aramid fiber, 1-1.5 parts of calcium lignin sulfonate, 10-20 parts of cationic chloroprene rubber latex, 20-30 parts of EVA emulsion and 120-200 parts of water. The preparation method of the acrylic acid grafted glass fiber includes the following steps: The glass fiber, acrylic acid and silane coupling agent are mixed in a mass ratio of 1: (0.2-0.3): (0.1-0.15), reacted at 80-90°C for 6-8h, washed, filtered and dried to obtain acrylic acid grafted glass fiber, wherein the silane coupling agent is a mixture of (N-anilino) methyltriethoxysilane and diethylaminomethyltriethoxysilane in a mass ratio of 1: (1.6-2); The preparation method of the dopamine-grafted aramid fiber comprises the following steps: The aramid fiber is immersed in acetone, washed, dried, immersed in potassium permanganate solution, washed, dried, and immersed in dopamine mixed solution, washed, and dried to obtain dopamine-grafted aramid fiber; the dopamine mixed solution contains diethylenetriaminepropyltrimethoxysilane and dopamine hydrochloride.
2. A composite high-strength concrete according to claim 1, characterized in that: The acrylic acid is a water-based hydroxy acrylic acid dispersion.
3. The composite high-strength concrete according to claim 1, characterized in that: The concentration of dopamine hydrochloride in the dopamine mixed solution is 20-30 g / L.
4. The composite high-strength concrete according to claim 1, characterized in that: The concentration of diethylenetriaminopropyltrimethoxysilane in the dopamine mixed solution is 7-10 g / L.
5. A process for preparing the composite high-strength concrete according to any one of claims 1 to 4, characterized in that: The steps include: S1. Screening coarse aggregate and fine aggregate to obtain aggregate; S2, mixing and crushing fly ash, slag, mineral powder and silicon powder to obtain crushed material; S3. Mix cement, aggregate, crushed material, acrylic acid grafted glass fiber, dopamine grafted aramid fiber, calcium lignin sulfonate, cationic chloroprene rubber latex, EVA emulsion and water to obtain composite high-strength concrete.
6. A process for preparing composite high-strength concrete according to claim 5, characterized in that: The particle size of the coarse aggregate is 8-10 mm.