A lithium ion battery electrolytic copper foil anti-oxidation liquid and preparation method thereof

By forming an organic-inorganic composite film on the surface of electrolytic copper foil in lithium-ion batteries, the problem of low high-temperature oxidation resistance of electrolytic copper foil in lithium-ion batteries is solved, and the high-temperature oxidation resistance and conductivity of electrolytic copper foil are improved.

CN116333545BActive Publication Date: 2024-11-22GUANGDONG TONGHE NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310286625.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-11-22
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

In existing technologies, the high-temperature oxidation resistance of electrolytic copper foil in lithium-ion batteries is low, which affects battery performance.

Method used

An anti-oxidation solution consisting of polymers, cyclohexanehexaphosphate, glucose, lithium saponite, sodium tungstate, and graphene oxide is used to form an organic-inorganic composite film through stirring, thereby improving the high-temperature anti-oxidation properties of electrolytic copper foil.

Benefits of technology

A uniform organic-inorganic composite film is formed on the surface of electrolytic copper foil, which improves the high-temperature oxidation resistance and conductivity of electrolytic copper foil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004148379680000051
    Figure BDA0004148379680000051
  • Figure BDA0004148379680000061
    Figure BDA0004148379680000061
Patent Text Reader

Abstract

The present invention provides an anti-oxidation liquid for electrolytic copper foil of lithium ion battery and a preparation method thereof, belonging to the technical field of surface treatment of electrolytic copper foil. The specific composition of the anti-oxidation liquid for electrolytic copper foil of lithium ion battery of the present invention is: 6 to 15 parts of polymer, 3 to 6 parts of cyclohexane hexaphosphate, 2 to 4 parts of glucose, 1 to 3 parts of laponite, 8 to 12 parts of sodium tungstate, 0.5 to 2.5 parts of graphene oxide, and 90 to 110 parts of water. The organic polymer, inorganic substance and organic ligand in the anti-oxidation liquid for electrolytic copper foil of lithium ion battery of the present invention cooperate with each other, so that a uniform organic-inorganic composite film is formed on the surface of the electrolytic copper foil, which can improve the high-temperature oxidation resistance of the electrolytic copper foil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of surface treatment of electrolytic copper foil, and in particular to an anti-oxidation liquid for electrolytic copper foil of a lithium ion battery and a preparation method thereof. Background Art

[0002] Electrolytic copper foil is a key material for lithium-ion batteries. Its performance directly affects the performance of lithium-ion batteries. In recent years, the lithium-ion battery industry has developed rapidly, and higher requirements have been placed on the performance of electrolytic copper foil. In the process of electrolytic copper foil, anti-oxidation treatment is a very important process. Oxidation and discoloration on the surface of copper foil not only affects the appearance of copper foil, but more importantly, it causes the adhesion of copper foil to decrease and copper foil spots to appear, which will affect the capacity and cycle stability of lithium-ion batteries.

[0003] Chinese patent application 201811101186.4 discloses a chromium-free anti-oxidation liquid and a water-free anti-oxidation process for electrolytic copper foil, which contains 5-9 g / L sodium tungstate, 1-3 g / L hydroxyethylidene diphosphonic acid, 4-7 g / L disodium ethylenediaminetetraacetic acid, and 1-3 mL / L phosphoric acid. The anti-oxidation liquid does not contain chromium, which is carcinogenic to humans, and zinc, which reduces battery performance. It can form a uniform polymer complex film on the surface of electrolytic copper. The copper foil may be slightly oxidized after baking at 140°C for 15 minutes. For example, Chinese invention patent publication number CN107634228A discloses a chromium-free anti-oxidation technology for electrolytic copper foil for lithium-ion batteries. After the original electrolytic copper foil is peeled off by the cathode roller, it enters the low-temperature anti-oxidation passivation liquid through the guide roller, soaks in it, squeezes it dry with the squeeze roller, and is directly rolled up after being blown dry by a high-pressure air knife at room temperature. The chromium-free anti-oxidation liquid contains 0.2-2.0 g / L of benzotriazole, 0.1-1.2 g / L of benzoic acid and 0.1-1.0 g / L of propyl acetate, with the remainder being deionized water. However, the high-temperature anti-oxidation performance of the chromium-free anti-oxidation liquid is poor, and partial or slight oxidation will occur after baking at 150°C for 30 minutes.

[0004] It can be seen that the high-temperature oxidation resistance of the copper foil treated with anti-oxidation in the prior art is low, so it is of great significance to provide a high-temperature anti-oxidation liquid for lithium-ion battery electrolytic copper foil and a preparation method thereof. Summary of the invention

[0005] The object of the present invention is to provide an anti-oxidation liquid for electrolytic copper foil of lithium ion battery and a preparation method thereof, so as to solve the technical problem of low high-temperature anti-oxidation performance of electrolytic copper foil of lithium ion battery in the prior art.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The invention provides a lithium ion battery electrolytic copper foil anti-oxidation liquid, comprising the following components in parts by weight: 6 to 15 parts of a polymer, 3 to 6 parts of cyclohexanehexol hexaphosphate, 2 to 4 parts of glucose, 1 to 3 parts of laponite, 8 to 12 parts of sodium tungstate, 0.5 to 2.5 parts of graphene oxide, and 90 to 110 parts of water.

[0008] Preferably, the polymer comprises polyacrylic acid and / or polyglutamic acid.

[0009] Preferably, the polymer is a mixture of polyacrylic acid and polyglutamic acid, wherein the mass ratio of polyacrylic acid to polyglutamic acid is 1 to 3:1.

[0010] Preferably, the pH value of the lithium-ion battery electrolytic copper foil anti-oxidation solution is 2-4.

[0011] The present invention provides a method for preparing an anti-oxidation liquid for electrolytic copper foil of a lithium ion battery, comprising the following steps:

[0012] (1) mixing a polymer, cyclohexanehexol hexaphosphate and glucose in 1 / 2 water to obtain a mixture;

[0013] (2) The lithium laponite, sodium tungstate, graphene oxide and the mixed material are sequentially mixed into the remaining 1 / 2 of water to obtain the lithium ion battery electrolytic copper foil anti-oxidation liquid.

[0014] Preferably, in step (1), the mixing is carried out under stirring conditions, wherein the stirring speed is 800-1200 rpm, the stirring time is 100-120 min, and the stirring temperature is 30-60°C.

[0015] Preferably, in step (2), the mixing is carried out under stirring conditions, wherein the stirring speed is 600 to 800 rpm and the stirring time is 30 to 60 min.

[0016] Beneficial effects of the present invention:

[0017] (1) The polymer in the anti-oxidation liquid for the electrolytic copper foil of the lithium ion battery of the present invention has a multifunctional functional group, which can form an organic film on the surface of the electrolytic copper foil. In addition, the organic polymer, the inorganic substance and the organic ligand cooperate with each other, so that a uniform organic-inorganic composite film is formed on the surface of the electrolytic copper foil, which can improve the high-temperature oxidation resistance of the electrolytic copper foil.

[0018] (2) The lithium laponite added to the anti-oxidation liquid of the lithium ion battery electrolytic copper foil of the present invention can ensure the high-temperature anti-oxidation property of the electrolytic copper foil to a certain extent while also having a high conductivity. DETAILED DESCRIPTION

[0019] The invention provides a lithium ion battery electrolytic copper foil anti-oxidation liquid, comprising the following components in parts by weight: 6 to 15 parts of a polymer, 3 to 6 parts of cyclohexanehexol hexaphosphate, 2 to 4 parts of glucose, 1 to 3 parts of laponite, 8 to 12 parts of sodium tungstate, 0.5 to 2.5 parts of graphene oxide, and 90 to 110 parts of water.

[0020] In the present invention, the weight content of the polymer is preferably 7 to 14 parts, and more preferably 8 to 13 parts; the weight content of the cyclohexanehexol hexaphosphate is preferably 4 to 5 parts, and more preferably 4 parts; the weight content of the glucose is preferably 2.5 to 3.5 parts, and more preferably 3 parts; the weight content of the laponite is preferably 1.5 to 2.5 parts, and more preferably 2 parts; the weight content of the sodium tungstate is preferably 9 to 11 parts, and more preferably 11 parts; the weight content of the graphene oxide is preferably 1 to 2 parts, and more preferably 1 part; the weight content of the water is 95 to 105 parts, and more preferably 100 parts.

[0021] In the present invention, the polymer comprises polyacrylic acid and / or polyglutamic acid.

[0022] In the present invention, the polymer is preferably a mixture of polyacrylic acid and polyglutamic acid, wherein the mass ratio of polyacrylic acid to polyglutamic acid is 1 to 3:1, preferably 1.5 to 2.5:1, and more preferably 2:1.

[0023] In the present invention, the pH value of the lithium ion battery electrolytic copper foil anti-oxidation liquid is 2-4, preferably 3.

[0024] The present invention provides a method for preparing an anti-oxidation liquid for electrolytic copper foil of a lithium ion battery, comprising the following steps:

[0025] (1) mixing a polymer, cyclohexanehexol hexaphosphate and glucose in 1 / 2 water to obtain a mixture;

[0026] (2) The lithium laponite, sodium tungstate, graphene oxide and the mixed material are sequentially mixed into the remaining 1 / 2 of water to obtain the lithium ion battery electrolytic copper foil anti-oxidation liquid.

[0027] In the present invention, in the step (1), mixing is carried out under stirring conditions, wherein the stirring speed is 800-1200 rpm, preferably 900-1100 rpm, and more preferably 1000 rpm; the stirring time is 100-120 min, preferably 105-115 min, and more preferably 110 min; the stirring temperature is 30-60°C, preferably 35-55°C, and more preferably 40-50°C.

[0028] In the present invention, in the step (2), mixing is carried out under stirring conditions, wherein the stirring speed is 600 to 800 rpm, preferably 650 to 750 rpm, and more preferably 700 rpm; the stirring time is 30 to 60 min, preferably 35 to 55 min, and more preferably 40 to 50 min.

[0029] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0030] Example 1

[0031] 3 parts of polyacrylic acid, 3 parts of polyglutamic acid, 3 parts of cyclohexanehexol hexaphosphate, 3 parts of glucose and 50 parts of water are mixed at 60°C with a stirring speed of 1000 rpm and a stirring time of 100 min to obtain a mixture; 1 part of lithium ore, 12 parts of sodium tungstate, 2.5 parts of graphene oxide and the mixture are sequentially added to the remaining 50 parts of water for mixing with a stirring speed of 600 rpm and a stirring time of 30 min to obtain a lithium ion battery electrolytic copper foil anti-oxidation liquid with a pH value of 3.5.

[0032] Example 2

[0033] 4 parts of polyacrylic acid, 2 parts of polyglutamic acid, 3 parts of cyclohexanehexol hexaphosphate, 3 parts of glucose and 50 parts of water are mixed at 50°C with a stirring speed of 1200 rpm and a stirring time of 120 min to obtain a mixture; 1 part of lithium ore, 12 parts of sodium tungstate, 2.5 parts of graphene oxide and the mixture are sequentially added to the remaining 50 parts of water for mixing with a stirring speed of 700 rpm and a stirring time of 60 min to obtain a lithium ion battery electrolytic copper foil anti-oxidation liquid with a pH value of 4.

[0034] Example 3

[0035] 10 parts of polyacrylic acid, 5 parts of polyglutamic acid, 5 parts of cyclohexanehexol hexaphosphate, 4 parts of glucose and 50 parts of water are mixed at 30°C, with a stirring speed of 800 rpm and a stirring time of 110 min to obtain a mixture; then 2 parts of lithium ore, 8 parts of sodium tungstate, 1 part of graphene oxide and the mixture are sequentially added to the remaining 50 parts of water for mixing, with a stirring speed of 800 rpm and a stirring time of 40 min to obtain a lithium ion battery electrolytic copper foil anti-oxidation liquid with a pH value of 3.

[0036] Example 4

[0037] 7.5 parts of polyacrylic acid, 2.5 parts of polyglutamic acid, 6 parts of cyclohexanehexol hexaphosphate, 2 parts of glucose and 50 parts of water are mixed at 40°C, wherein the stirring speed is 900 rpm and the stirring time is 100 min to obtain a mixture; then 3 parts of lithium ore, 10 parts of sodium tungstate, 0.5 parts of graphene oxide and the mixture are sequentially added to the remaining 50 parts of water for mixing, and the mixing is carried out under stirring conditions, the stirring speed is 600 rpm, and the stirring time is 30 min to obtain a lithium ion battery electrolytic copper foil anti-oxidation liquid with a pH value of 2.

[0038] Comparative Example 1

[0039] 10 parts of polyacrylic acid, 6 parts of cyclohexanehexol hexaphosphate, 2 parts of glucose and 50 parts of water are mixed at 40°C, with a stirring speed of 900 rpm and a stirring time of 100 min to obtain a mixture; then 3 parts of lithium ore, 10 parts of sodium tungstate, 0.5 parts of graphene oxide and the mixture are sequentially added to the remaining 50 parts of water for mixing, with a stirring speed of 600 rpm and a stirring time of 30 min to obtain a lithium ion battery electrolytic copper foil anti-oxidation liquid with a pH value of 3.

[0040] Comparative Example 2

[0041] 7.5 parts of polyacrylic acid, 2.5 parts of polyglutamic acid, 6 parts of cyclohexanehexol hexaphosphate, 2 parts of glucose and 50 parts of water are mixed at 40°C with a stirring speed of 900 rpm and a stirring time of 100 min to obtain a mixture; 10 parts of sodium tungstate, 0.5 parts of graphene oxide and the mixture are sequentially added to the remaining 50 parts of water for mixing with a stirring speed of 600 rpm and a stirring time of 30 min to obtain a lithium ion battery electrolytic copper foil anti-oxidation liquid with a pH value of 2.5.

[0042] Comparative Example 3

[0043] 7.5 parts of polyacrylic acid, 2.5 parts of polyglutamic acid, 6 parts of cyclohexanehexol hexaphosphate, 2 parts of glucose and 50 parts of water are mixed at 40°C, with a stirring speed of 900 rpm and a stirring time of 100 min to obtain a mixture; 10 parts of sodium tungstate and the mixture are sequentially added to the remaining 50 parts of water for mixing, with a stirring speed of 600 rpm and a stirring time of 30 min to obtain a lithium ion battery electrolytic copper foil anti-oxidation liquid with a pH value of 3.

[0044] Comparative Example 4

[0045] 6 parts of cyclohexanehexol hexaphosphate, 2 parts of glucose and 50 parts of water are mixed at 40°C with a stirring speed of 900 rpm and a stirring time of 100 min to obtain a mixture; 3 parts of tungsten-lithium stone, 10 parts of sodium tungstate, 0.5 parts of graphene oxide and the mixture are sequentially added to the remaining 50 parts of water for mixing with a stirring speed of 600 rpm and a stirring time of 30 min to obtain a lithium-ion battery electrolytic copper foil anti-oxidation liquid with a pH value of 4.

[0046] Performance Test:

[0047] The process of anti-oxidation treatment of electrolytic copper foil using the anti-oxidation liquid prepared in Examples 1 to 4 and Comparative Examples 1 to 4 includes the following steps: the original copper foil is peeled off by the lower guide roller, and then immersed in the anti-oxidation liquid through the guide roller, the temperature of the anti-oxidation liquid is controlled to be 35°C, the immersion time is 20s, and then squeezed dry by the upper guide roller, and directly rolled up after being blown dry with a 0.8kPa wind knife at room temperature, and the anti-oxidation treatment is completed. Table 1 shows the performance test results of the copper foil treated with the anti-oxidation liquid prepared in Examples 1 to 4 and Comparative Examples 1 to 4.

[0048] Table 1 Performance test results of copper foil after anti-oxidation treatment

[0049]

[0050]

[0051] The test results in Table 1 are analyzed. By comparing the data of Example 4 with Comparative Example 1, it can be concluded that the cooperation between polyacrylic acid and polyglutamic acid can improve the high-temperature oxidation resistance of copper foil; by comparing the data of Example 4 with Comparative Examples 2 and 3, it can be concluded that the addition of graphene oxide and hectorite can reduce the resistivity of copper foil and improve the conductivity of copper foil; by comparing the data of Example 4 with Comparative Example 4, it can be concluded that the addition of polymer can cooperate with inorganic substances to form an organic-inorganic composite film that can further improve the high-temperature oxidation resistance of copper foil.

[0052] It can be seen from the above embodiments that the present invention provides a lithium ion battery electrolytic copper foil anti-oxidation liquid and a preparation method thereof, which specifically comprises: 6 to 15 parts of polymer, 3 to 6 parts of cyclohexane hexaphosphate, 2 to 4 parts of glucose, 1 to 3 parts of hectorite, 8 to 12 parts of sodium tungstate, 0.5 to 2.5 parts of graphene oxide, and 90 to 110 parts of water. The organic polymer, inorganic substance and organic ligand in the lithium ion battery electrolytic copper foil anti-oxidation liquid of the present invention cooperate with each other, so that a uniform organic-inorganic composite film is formed on the surface of the electrolytic copper foil, which can further improve the high-temperature oxidation resistance of the electrolytic copper foil.

[0053] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A lithium ion battery electrolytic copper foil anti-oxidation solution, characterized in that: The invention is prepared from the following components in parts by weight: 6 to 15 parts of polymer, 3 to 6 parts of cyclohexane hexol hexaphosphate, 2 to 4 parts of glucose, 1 to 3 parts of laponite, 8 to 12 parts of sodium tungstate, 0.5 to 2.5 parts of graphene oxide, and 90 to 110 parts of water; The polymer is prepared by mixing polyacrylic acid and polyglutamic acid, wherein the mass ratio of polyacrylic acid to polyglutamic acid is 1-3:

1.

2. The lithium ion battery electrolytic copper foil anti-oxidation solution according to claim 1, characterized in that: The pH value of the lithium ion battery electrolytic copper foil anti-oxidation liquid is 2-4.

3. The method for preparing the anti-oxidation liquid for electrolytic copper foil of lithium ion battery according to claim 1 or 2, characterized in that: The following steps are involved: (1) mixing a polymer, cyclohexanehexol hexaphosphate and glucose in 1 / 2 water to obtain a mixture; (2) The lithium laponite, sodium tungstate, graphene oxide and the mixed material are sequentially mixed into the remaining 1 / 2 of water to obtain the lithium ion battery electrolytic copper foil anti-oxidation liquid.

4. The preparation method according to claim 3, characterized in that: In the step (1), the mixing is carried out under stirring conditions, wherein the stirring speed is 800-1200 rpm, the stirring time is 100-120 min, and the stirring temperature is 30-60°C.

5. The preparation method according to claim 3 or 4, characterized in that: In the step (2), the mixing is carried out under stirring conditions, wherein the stirring speed is 600 to 800 rpm and the stirring time is 30 to 60 minutes.