Anti-fatigue coated steel plate and production method thereof
A fatigue-resistant coated steel plate with a tailored composition and production process addresses the corrosion and fatigue challenges of marine structures in tropical and subtropical waters, enhancing durability and resistance to environmental stress.
Patent Information
- Application Number
- CN202211610417.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-12-14
AI Technical Summary
Marine structures in tropical and subtropical waters face severe corrosion and fatigue issues due to harsh environmental factors, leading to premature failure and high economic losses, with existing materials lacking adequate fatigue resistance and corrosion protection, especially under strong storms and large wave loads.
A fatigue-resistant coated steel plate with a specific composition and microstructure, including elements like C, Si, Mn, Mg, Ca, V, N, Cu, Ni, Mo, Re, Cr, REM, Sn, P, and S, combined with a production process involving smelting, continuous casting, and controlled rolling, to enhance corrosion resistance and mechanical properties.
The steel plate exhibits improved corrosion resistance and fatigue life, with a corrosion resistance 90-150% higher than 3.5Ni system steel, maintaining integrity under extreme conditions and supporting high operational cycles without failure.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal material preparation, and particularly relates to an anti-fatigue coated steel plate and a production method thereof. Background Art
[0002] Tropical and subtropical seas have unique characteristics of high temperature (ocean surface temperature 25-28℃, up to 30℃), high salt (Cl - Deposition rate 1.12mg / 100cm 2 d or above), strong storms (maximum wave height of nearly 30m), and other strong corrosive and fatigue damage environmental factors. The natural environment is harsh and the material corrosion problem is very prominent. According to the ISO9223 classification standard, the corrosion level of materials in this area can reach the highest level C5. Compared with other regions, surface ships, offshore floating platforms, island and reef buildings, equipment and facilities currently serving in this environment will suffer from severe corrosion prematurely even if corrosion protection measures are taken. According to statistics, the failure rate of equipment and facilities serving in tropical and subtropical waters is three times that of other waters, causing nearly 1 trillion yuan of economic losses to the country every year. The tropical and subtropical marine environment includes island and reef construction, resource mining platforms, marine life auxiliary equipment, marine clean energy development equipment, etc., mainly steel structures. It is estimated that the steel consumption in tropical and subtropical waters will reach 1 million tons / year in the next 5-10 years.
[0003] In addition to facing the harsh and complex marine environment of high salt and high temperature during service, marine engineering structures in tropical and subtropical waters are often subjected to environmental loads such as sea breeze, waves and currents, as well as repeated effects of operational dynamic loads. For example, an offshore platform with a design life of 20-25 years may experience hundreds of millions of cycles of alternating stress caused by wave action during its service life. In addition, marine environment construction engineering structures, especially offshore platforms, often have to support various equipment with a total mass of hundreds of tons, which causes them to be subjected to extremely high working stress. In addition, due to their large size and thickness, joint defects such as microcracks, pores, slag inclusions, and unfused joints can easily become sources of cracks for corrosion and fatigue, resulting in reduced fatigue toughness. Therefore, fatigue issues must also be considered during the use of marine engineering structures and their service. At present, the research and development of special materials for the harsh environment of four highs and one strong in my country's tropical and subtropical waters is not systematic, and related research is mainly carried out on the corrosion resistance of materials. The domestic patent application number 201710075154.0 is a high-corrosion-resistant low-alloy steel suitable for high-temperature coastal environments. Its corrosion resistance is better than that of Q235 carbon steel and other weathering steels. Due to the use of a high Ni system and alloying with elements such as Cu and Mo, the problem is that the cost is high, and due to the high alloying and carbon equivalent, there are problems with welding performance; in addition, the yield strength of this system steel is often 600-800MPa, and the fatigue problem of steel is prominent, resulting in a large safety hazard; in addition, for some extremely harsh coastal construction environments and applications with coating requirements, the local failure and corrosion caused by the damage and aging of the coating, as well as the fatigue corrosion problem are extremely harmful, which is particularly important for the long-term serviceability of the combined use system of steel + coating. Not only does it require good corrosion resistance of the steel, but it also requires the steel-coating interface system to have a high corrosion resistance. Currently, there are no reports on fatigue-resistant coated steels for materials under severe corrosion, strong storms, and large wave load conditions in tropical and subtropical waters. Summary of the invention
[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide an anti-fatigue coated steel plate and a production method thereof, which has an anti-fatigue coated steel with higher safety in service and solves the fatigue-corrosion coupling problem faced by marine structures under strong storms and large wave loads.
[0005] In order to solve the above problems, the technical solution adopted by the present invention is as follows: a fatigue-resistant coating steel plate, wherein the steel composition is calculated by weight percentage: C: ≤ 0.02wt%, Si: 0.3-0.45wt%, Mn: 0.4-0.6wt%, Mg: 0.005-0.01wt%, Ca: 0.008-0.015wt%, V: 0.04-0.06wt%, N: 0.008-0.012wt%, Cu: 0 .2-0.4wt%, Ni: 1-2wt%, Mo: 0.05-0.1wt%, Re: 0.03-0.04wt%, Cr: 1-1.5wt%, REM: 0.03-0.05wt%, Sn: 0.25-0.35wt%, P: 0.01-0.015wt%, S: ≤0.005wt%, Ti: 0.001-0.005wt%, the balance is Fe and unavoidable impurities.
[0006] Furthermore, the steel plate contains 55-70% bainite + 25-35% ferrite (including 7-12% acicular ferrite) structure, and the percentage is area percentage; it contains V (C, N) and Mo2C nanophases with an average size of 15-25nm dispersed and precipitated, and the average spacing between these phases is 1.2-1.5μm; it contains Cu nanophases with an average size of 25-45nm, and the average spacing between the phases is 1.1-1.6μm.
[0007] Furthermore, the steel plate matrix contains dispersed precipitated V (C, N) and Mo2C with a size of 10-40 nm, and the size of the Cu nanophase is 25-60 nm.
[0008] Furthermore, the average grain size of the surface layer -1 / 8 of the thickness of the steel plate is 10-20 μm.
[0009] Furthermore, the steel plate has a yield strength of 420-460 MPa, a yield strength ratio of ≤0.75, an impact energy of not less than 190 J at -40°C, an elongation of ≥20%, and a cross-sectional shrinkage of ≥68%.
[0010] Furthermore, the steel plate has a loading stress ratio of 0.1, a frequency of 90HZ, and a maximum stress of 0.75Rp. 0.2 When the number of cycles reaches 10 7 The sample does not break, -20℃CTODδm>0.8mm.
[0011] The second technical solution of the present invention is a method for producing a fatigue-resistant coated steel plate, including smelting, continuous casting, billet heating, controlled rolling and offline processing, and the specific contents are as follows:
[0012] Billet heating: The temperature of the cold billet into the furnace is controlled at 50-100℃, and multi-stage heating is adopted. The total time of 500-900℃ is controlled within 0.1-0.2min / mm, the total time of 1150-1180℃ is controlled within 0.1min / mm, and the total time of the soaking section 1120-1150℃ is controlled within 0.2-0.4min / mm;
[0013] Controlled rolling: After the billet is taken out of the furnace, the temperature is raised to 950-1000℃ before rolling. The final rolling temperature is controlled above 900℃. The reduction per pass in this stage is controlled at 20-30%, and the cooling rate after rolling is controlled at 3-7℃ / s.
[0014] Off-line treatment: After the steel plate is off the line, the second stage precipitation phase and internal stress are regulated by thermal insulation treatment, and the thermal insulation regulation temperature is 320-390℃.
[0015] Furthermore, the steel billet is made by converter smelting + continuous casting, and is pre-treated by rapid cooling when it is discharged. The surface temperature of the initial cooling is controlled at 815-890°C, and the cooling rate is controlled at 2-8°C / s. Thereafter, low-temperature heating treatment is adopted, and the treatment temperature is 220-370°C.
[0016] Furthermore, the steel is smelted in a converter, the Ti element in the molten iron is controlled below 0.005%, and Si and Mn are used for deoxidation.
[0017] The anti-fatigue coated steel produced according to the above scheme has the following beneficial effects:
[0018] 1. The corrosion resistance of the steel plate is greatly improved by adding and synergizing composite trace elements. Using a simulated tropical and subtropical seawater splash zone immersion test, the corrosion resistance of the steel plate coating system is 90-150% higher than that of 3.5Ni system steel.
[0019] 2. It has good comprehensive mechanical properties, structural safety and weldability, with yield strength of 420-460Mpa, yield strength ratio ≤0.75, impact energy at -40℃ not less than 190J, elongation ≥20%, and section shrinkage ≥68%.
[0020] 3. Loading stress ratio is 0.1, frequency is 90HZ, and the maximum stress is 0.75Rp 0.2 When the number of cycles reaches 10 7 The sample does not break, -20℃CTODδm>0.8mm DETAILED DESCRIPTION
[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other examples improved or modified by ordinary technicians in this field belong to the scope of protection of the present invention. It should be understood that the embodiments of the present invention are only used to illustrate the technical effects of the present invention, rather than to limit the scope of protection of the present invention.
[0022] The present invention is aimed at the steel materials facing high temperature, unstable oxygen, low pH value, high Cl - In a more complex environment, the pH value of the anode area is reduced through the microalloying and compounding of elements such as Sn, Re, REM, N, V, Cr, W, Ca, Mg, and Sb, thereby increasing the system potential, reducing the local pH value, and improving the coupled passivation ability of the steel-coating system. The developed steel plate has good comprehensive performance of mechanical-corrosion resistance matching, coupled corrosion resistance of the coating, and high fatigue resistance. Using a simulated tropical and subtropical seawater splash zone immersion test, the corrosion resistance of the steel plate's coating system is 90-150% higher than that of 3.5Ni system steel, effectively solving the fatigue failure problem faced by deep-sea coating equipment in marine environments.
[0023] The steel composition of the present invention will be described in detail below. Unless otherwise specified, the content of each element is expressed in % by weight.
[0024] The invention discloses an anti-fatigue coating steel plate, wherein the steel composition is, by weight percentage, C:≤0.02wt%, Si: 0.3-0.45wt%, Mn: 0.4-0.6wt%, Mg: 0.005-0.01wt%, Ca: 0.008-0.015wt%, V: 0.04-0.06wt%, N: 0.008-0.012wt%, Cu: 0.2-0.4wt%, Ni: 1-2wt%, Mo: 0.05-0.1wt%, Re: 0.03-0.04wt%, Cr: 1-1.5wt%, REM: 0.03-0.05wt%, Sn: 0.25-0.35wt%, P: 0.01-0.015wt%, S:≤0.005wt%, Ti: 0.001-0.005wt%, and the balance is Fe and unavoidable impurities.
[0025] C:≤0.02wt%
[0026] The C element is the main phase change controlling element for forming a corrosion-resistant structure with 55-70% bainite + 25-35% ferrite (including 7-12% acicular ferrite) as the matrix, and is an important element for ensuring the strength of the steel grade. Appropriate C promotes the formation of the important micro cathode phase V (C, N) in the present invention and controls the precipitation of large carbides of Cr. These phases help to improve the corrosion resistance of the steel. Under the component system of the present invention, more C is not good for the corrosion resistance of the steel, so the C content should be ≤0.03wt%. Considering the adverse effect of C on weldability, C is further controlled to be ≤0.02wt%.
[0027] Si: 0.3-0.45wt%
[0028] The Si element plays a certain role in strengthening and is one of the important deoxidizers of the present invention. It can promote the surface enrichment of Sn and form surface oxides with Cu and Sn, effectively improving the corrosion resistance. Appropriate Si helps to improve the potential of the coating system and control the local pH value, so the Si content is controlled at 0.3-0.45wt%;
[0029] Mn: 0.4-0.6wt%
[0030] The Mn element plays a certain role in the composite control of strengthening and fatigue properties, and is one of the important deoxidizers of the present invention. Too much Mn will reduce the corrosion resistance of the steel and affect the solid solution effect of the corrosion-resistant elements in the steel. Therefore, the Mn content is controlled at 0.4-0.6wt%;
[0031] Mg: 0.005-0.01wt%; Ca: 0.008-0.015wt%
[0032] The Ca and Mg elements are mainly used to reduce the cathode reaction area and the pH value under the coating, which plays a passivation role in protecting Cr; in addition, trace amounts of Ca and Mg dissolved in Fe can make Ni, Cu, Cr, Sn and other corrosion-resistant elements relatively enriched after the surface Fe dissolves in the early stage of corrosion, improve corrosion resistance, and reduce the toughness reduction problem caused by the addition of high Sn and other elements. The above elements will also form a coupling effect with Zn in the primer in a weakly acidic environment to improve the corrosion resistance of the steel-coating system. Based on the above design, the content of Ca and Mg elements is controlled at 0.008-0.015wt% and 0.005-0.01wt% respectively;
[0033] V: 0.04-0.06wt%
[0034] The V element plays an important role in the toughness and corrosion resistance of steel mainly in the form of precipitation strengthening. The role of V in the present invention is mainly to form V (C, N) with appropriate proportions of C and N. Since the steel material is a multiphase structure formed by multi-element alloying, the control of the cathode ratio in the micro-region is very important. The refined, dispersed, uniform and distributed cathode design is very important for controlling the corrosion resistance of the complex structural system of the steel material. Based on this, the present invention adopts a trace amount of 0.04-0.06wt% of V to give full play to its excellent precipitation effect. The electrochemical impedance spectrum shows that after full precipitation, the surface inductive arc of the steel grade is greatly weakened, indicating that the pitting phenomenon is effectively suppressed. It mainly plays the role of controlling the cathode phase. Under the configuration of V, C, N and Cr elements adopted in the present invention, it will promote the generation of 10-40nm dispersed precipitation V (C, N) in the steel matrix, with an average spacing of 1.2-1.5μm, mainly in spherical shape, which can further prevent the expansion of fatigue cracks. Based on the above design, the content of V is 0.04-0.06wt%;
[0035] N: 0.008-0.012wt%;
[0036] The N element mainly promotes the composite precipitation of fine particles of V (C, N) and Fe3C. In addition, the solid-dissolved N helps to improve the corrosion resistance of steel.
[0037] Cu: 0.2-0.4wt%;
[0038] Cu is an important corrosion-resistant and toughening element of the present invention. On the one hand, in the early stage of corrosion, when the surface is initially corroded, an enrichment layer and an oxide layer are formed, which improves the lack of significant segregation behavior. In addition, a nanophase with an average size of 25-45nm is formed inside the steel plate, and the average spacing between the phases is 1.1-1.6μm. After the surface rust layer is destroyed, a large number of fine cathode phases are further formed to form a unique cathode size and distribution control system with V (C, N) and Fe3C, which controls the corrosion rate and helps to improve and control the weldability. However, too much Cu is not conducive to further exertion of corrosion resistance and increases unnecessary costs. Therefore, the Cu content of the present invention is controlled at 0.2-0.4wt%;
[0039] Ni: 1-2wt%;
[0040] The main function of Ni element is to balance the toughness of weathering steel. In terms of corrosion resistance, it promotes the positive movement of the self-corrosion potential on the steel surface. The present invention adopts a low Mn component design, so that Ni can more effectively promote the formation of Fe3O4 oxides, and Ni in the rust layer 2+ It can more effectively occupy the interstitial position of Fe3O4, forming a stable and dense intermetallic compound of Fe and Ni, preventing Cl -Diffusion into the matrix reduces acidification and increases the pH value of the electrolyte in the rust layer, so that only 1-2wt% Ni can fully achieve the corrosion resistance.
[0041] Mo: 0.05-0.1wt%;
[0042] Mo element can make the rust layer dense, and when combined with Si, Cu, etc., the oxide film formed is effective against initial corrosion. In addition, along with the anodic reaction of steel, MoO4 2- Dissolved, MoO4 on the rust layer 2- distribution, producing ion selection, resisting the corrosion promoting factor Cl - Intrusion. In addition, the addition of Mo helps to improve the low and high temperature stability of the V and Cu dispersed phases, and precipitates 10-40nm Mo2C, improving its pitting and fatigue resistance. Too high Mo will deteriorate the toughness, too low is not conducive to fatigue resistance, and too high is not conducive to the coupling effect between the coating and steel, so it is controlled at 0.05-0.1wt%;
[0043] Re: 0.03-0.04wt%;
[0044] The Re element is evenly distributed in the dendrite trunk and between dendrites during the solidification process. It is an important solid solution strengthening element. Its corrosion potential is about 0.3V, which can shift the corrosion potential positively, effectively increase the corrosion potential of the matrix, reduce the corrosion current of the system, and improve the corrosion resistance of steel. In addition, an appropriate amount of Re combined with Ni and Cu can effectively promote anode passivation and improve cathode efficiency. Since the anode current in the passivation zone is several orders of magnitude smaller than the current of activation and dissolution, it is very effective to use cathodic elements to improve the corrosion resistance of the alloy. In addition, the compound addition of Re, V, and Ni can effectively control the toughness control problems caused by the addition of elements such as Sn, and improve the bonding between steel and coating. Therefore, it is controlled at 0.03-0.04wt%;
[0045] Cr: 1-1.5wt%;
[0046] Cr; on the one hand, it plays the role of dense rust layer, on the other hand, it forms a passive oxide, which together with other oxides and dense α-FeOOH resists Cl - Intrusion; In addition, in the composition design of the multi-component system of the present invention, solid solution elements such as Cr are fully dissolved in the matrix, which reduces the solid solubility of V and improves its precipitation behavior, indirectly controlling the thermodynamic and kinetic changes of V (C, N), and after the compounding of Cr, V and other elements forms a stable rust layer, the inductive impedance effect tends to completely disappear, indicating that the material's fatigue resistance and pitting resistance have reached the best match. However, too much Cr is not conducive to the control of pH under the coating, so the Cr of the present invention is controlled at 1-1.5wt%.
[0047] REM: 0.03-0.05wt%;
[0048] On the one hand, REM rare earth elements can change the size of cathode phases such as V (C, N), increase their dispersion, increase their potential, and reduce their cathode effect. Because the content reaches 0.03-0.05wt%, it is fully dissolved in the matrix, which plays a role in increasing the matrix potential and directly produces corrosion resistance. The RE absorbed by grain boundaries, subgrain boundaries, precipitate mismatches and other positions plays a role in balancing the segregation of elements such as Cr and Cu, reducing intergranular and interphase corrosion caused by segregation.
[0049] Sn: 0.25-0.35wt%;
[0050] On the one hand, Sn element can reduce the energy level of steel and weaken the electrochemical activity of steel in the form of single substance solid solution. In addition, it helps to form oxides such as SnO and deposit on the corrosion front, promote the formation of α-FeOOH, and compact the oxide layer together with α-FeOOH. When dissolved with Fe, ionic Sn can react with Cl - Combined with the above, the local pH value is increased, the corrosion process is accelerated, and the local pH value is increased, especially the pH under the coating, which plays a role in controlling the acceleration of the corrosion process. The Sn content of the present invention is controlled at 0.25-0.35wt%.
[0051] P: 0.01-0.015wt%;
[0052] The P element is mainly used to reduce the degree of anode polarization, promote the uniform dissolution of steel and accelerate the oxidation rate of iron, promote the formation of non-static protective film, and cooperate with Re, Cu, etc. to resist Cl - Considering that too much P reduces the weldability of the coated steel to a certain extent, the P content of the present invention is controlled at 0.01-0.015wt%;
[0053] S: ≤0.005wt%;
[0054] S: Sulfides formed by elements accelerate corrosion and weaken toughness, so they need to be strictly controlled to ≤0.005wt%;
[0055] Ti: 0.001-0.005wt%
[0056] The Ti element helps to control the initial grain size, but too much will consume the N element, affecting the strength and corrosion resistance of the steel. Therefore, the Ti content of the present invention is controlled within 0.001-0.005 wt%.
[0057] In addition to the above-mentioned steel components, the balance of the present invention may be Fe and inevitable impurities. Inevitable impurities are impurities that are not artificially mixed in the general steel manufacturing process. They cannot be completely excluded, and the meaning can be easily understood by those skilled in the art of general steel manufacturing. In addition, the present invention does not completely exclude the addition of other components in addition to the above-mentioned steel components.
[0058] The microstructure of the present invention will be described in further detail below.
[0059] The invention discloses an anti-fatigue coating steel plate, wherein the matrix contains V (C, N) and Mo2C dispersed and precipitated with a size of 10-40nm (average size of 15-25nm), the average spacing of these phases is 1.2-1.5μm, and Cu nanophase with a size of 25-60nm (average size of 25-45nm), the average spacing of the phases is 1.1-1.6μm. After rolling, the steel plate forms a corrosion-resistant structure with 55-70% bainite + 25-35% ferrite (including 7-12% acicular ferrite) as the matrix, the percentage is the area percentage, and the average grain size of the surface layer-1 / 8 thickness of the steel plate is 10-20μm.
[0060] The production process of the present invention is described in further detail below.
[0061] A production method for anti-fatigue coated steel plate, including smelting, continuous casting, billet heating, controlled rolling and offline processing, the specific contents are as follows:
[0062] Smelting: The steel is smelted in a converter, and Si and Mn are used for deoxidation. The use of Al is strictly controlled because the addition of Al will consume the N element and have a harmful effect on the surface quality of the steel billet. Similarly, the introduction of Ti and Nb elements in the molten iron should also be strictly controlled (controlled to below 0.005%), which affects the precipitation effect of V and Cu and avoids the formation of Ti, Al, Nb and other carbonitrides, which is not conducive to corrosion resistance.
[0063] Continuous casting: In order to control the initial surface grain size of the continuous casting billet and the solid distribution of corrosion-resistant elements, rapid cooling is used for pretreatment when the billet is discharged. The surface temperature is controlled at 815-890℃ and the cooling rate is controlled at 2-8℃ / s. After that, hot charging is not suitable and low-temperature heating treatment is required. The treatment temperature is 220-370℃ to control the surface quality and thermal stress distribution of the billet.
[0064] Billet heating: The temperature of the billet cold-charged into the furnace is controlled at 50-100℃, and multi-stage heating is adopted. The total time of 500-900℃ is controlled within 0.1-0.2min / mm, the total time of 1150-1180℃ is controlled within 0.1min / mm, and the total time of the soaking section 1120-1150℃ is controlled within 0.2-0.4min / mm. The purpose is to control the initial distribution of alloy elements and trace elements before hot working. Since the distribution and composition of grains, especially grain boundaries, have a greater impact on corrosion, it is necessary to reasonably control the initial grain size.
[0065] Controlled rolling: high temperature controlled rolling with large reduction. Specifically, the billet is rolled after being heated to 950-1000℃ after being taken out of the furnace. The final rolling temperature is controlled at above 900℃. The reduction of each pass in this stage is controlled at 20-30%. After rolling, the austenite phase transformation zone is quickly passed by rapid cooling. The cooling rate is controlled at 3-7℃ / s. The purpose is to balance the phase transformation and grain size. The surface grain size is controlled, and the average grain size of the surface layer of the steel plate -1 / 8 thickness is controlled at 10-20μm. The distribution state of the surface corrosion-resistant elements is controlled, the precipitation of elements such as V, Cu, and Mo is suppressed, and the components in the steel are supercooled. In addition, the control of the surface grain size can ensure the balance of mechanical and corrosion resistance. The above process forms a corrosion-resistant structure with 55-70% bainite + 25-35% ferrite (including 7-12% acicular ferrite) as the matrix.
[0066] Off-line treatment: After the steel plate is off the line, the second stage of precipitation phase and internal stress are regulated by heat preservation treatment. Cooling improves the precipitation power of the fine phase. Low temperature regulation of 320-390℃ can be used. On the one hand, the surface hardness can be regulated to improve the mechanical properties of the steel plate surface. On the other hand, finer precipitates are formed to improve the overall corrosion resistance of the steel plate. After regulation, V (C, N) and Mo2C with a size of 10-40nm (average size 15-25nm) are dispersed and precipitated in the matrix of the steel. The average spacing of these phases is 1.2-1.5μm. At the same time, there are 25-60nm (average size 25-45nm) Cu nanophases in the matrix, and the average spacing of the phases is 1.1-1.6μm.
[0067] Aiming at the complex environment of strong corrosion and large wave loads faced by offshore building structures in tropical and subtropical waters, the present invention proposes a new component system design and corresponding production process. The developed steel grade takes into account strength and toughness, weldability, and yield strength ratio, and has good fatigue resistance and coating coupled service performance.
[0068] According to the above chemical composition and production process, the actual smelting composition of the present invention is shown in Table 1, the actual process parameters of the present invention are shown in Tables 2-5, and the actual properties are shown in Tables 6-10.
[0069] Table 1 Composition of each example (wt%)
[0070] C Si Mn Mg Ca V N Cu Ni Mo Re Cr REM Sn P S Ti 1 0.02 0.35 0.56 0.008 0.012 0.056 0.011 0.37 1.62 0.05 0.03 1.47 0.04 0.25 0.013 0.003 0.003 2 0.01 0.31 0.46 0.007 0.013 0.042 0.008 0.38 1.33 0.07 0.036 1.32 0.04 0.35 0.011 0.002 0.001 3 0.02 0.3 0.55 0.008 0.01 0.052 0.009 0.4 1.25 0.07 0.032 1.45 0.03 0.25 0.012 0.002 0.004 4 0.02 0.4 0.59 0.006 0.012 0.043 0.008 0.29 1.32 0.1 0.038 1.18 0.04 0.25 0.015 0.002 0.003 5 0.02 0.35 0.54 0.009 0.008 0.044 0.011 0.24 1.88 0.08 0.04 1.15 0.05 0.34 0.014 0.003 0.003 6 0.02 0.34 0.43 0.01 0.01 0.058 0.008 0.33 1.65 0.06 0.035 1.27 0.05 0.33 0.011 0.003 0.005 7 0.01 0.33 0.58 0.008 0.015 0.054 0.009 0.26 1.87 0.07 0.038 1.3 0.03 0.32 0.013 0.003 0.003 8 0.02 0.41 0.41 0.008 0.015 0.045 0.01 0.32 2 0.06 0.037 1.25 0.03 0.27 0.012 0.003 0.004 9 0.02 0.32 0.51 0.01 0.01 0.059 0.009 0.29 1.81 0.06 0.03 1.34 0.04 0.32 0.014 0.005 0.002 10 0.01 0.33 0.57 0.01 0.013 0.05 0.008 0.34 1.68 0.1 0.033 1.11 0.05 0.31 0.013 0.002 0.002
[0071] Table 2 Pretreatment of blanks
[0072]
[0073] Table 3 Heating process
[0074]
[0075] Table 4 Rolling process and microstructure control results
[0076]
[0077] Table 5 Steel plate off-line process technology and organizational proportion level
[0078]
[0079] Table 6 Mechanical properties of the examples
[0080]
[0081] Table 7 Fatigue properties of the examples
[0082]
[0083] Table 8 Welding performance of the embodiment (line energy 35KJ, submerged arc welding)
[0084]
[0085] The test steel and the comparison steel were protected by four layers of Zn-rich primer to make the coated steel accelerated corrosion coupons for the steel-coating accelerated corrosion test. The single test method was as follows:
[0086] 1. 42℃, relative humidity 90%, time 5h;
[0087] 2. Accelerated corrosion test simulating tropical and subtropical sea conditions was adopted, 2% NaCl solution: pH value: PH: 6-6.9, immersion temperature 42±2℃, time 1h;
[0088] 3. Exposure temperature 45±2℃, exposure humidity 60%, time 10h;
[0089] The number of times that 10% coating degradation (peeling of notched parts, bubbling, etc.) occurs after corrosion cycles is used as an evaluation of the corrosion resistance of the system. The number of corrosion cycles is 44 to 64, and the relative corrosion resistance is 194% to 252%.
[0090] Table 9 Corrosion resistance of the examples
[0091] Corrosion cycles Relative corrosion resistance Comparative Example (3.5Ni Steel) 33 100% Example 1 78 229% Example 2 71 208% Example 3 75 220% Example 4 79 232% Example 5 86 252% Example 6 69 203% Example 7 67 197% Example 8 66 194% Example 9 74 217% Example 10 70 205%
[0092] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A fatigue-resistant coated steel plate, characterized in that: The steel plate composition is calculated by weight percentage: C: ≤0.02 wt%, Si: 0.3-0.45wt%, Mn: 0.4-0.6wt%, Mg: 0.005-0.01 wt%, Ca: 0.008-0.015wt%, V: 0.04-0.06wt%, N: 0.008-0.012 wt%, Cu: 0.2-0.4 wt%, Ni: 1-2wt%, Mo: 0.05-0.1 wt%, Re: 0.03-0.04wt%, Cr: 1-1.5wt%, REM: 0.03-0.05 wt%, Sn: 0.25-0.35wt%, P: 0.01-0.015 wt%, S: ≤0.005wt%, Ti: 0.001-0.005wt%, and the balance is Fe and unavoidable impurities; The steel plate contains 55-70% bainite + 25-35% ferrite structure, 25-35% ferrite contains 7-12% acicular ferrite, and the percentages are area percentages; it contains V (C, N) and Mo2C nanophases with an average size of 15-25nm dispersed and precipitated, and the average spacing of these phases is 1.2-1.5μm, and contains Cu nanophases with an average size of 25-45nm, and the average spacing of the Cu nanophases is 1.1-1.6μm; The steel plate matrix contains dispersed precipitated V (C, N) and Mo2C with a size of 10-40nm, and the size of the Cu nanophase is 25-60nm; The average grain size of the steel plate surface layer - 1 / 8 thickness is 10-20μm.
2. The anti-fatigue coated steel plate according to claim 1, characterized in that: The steel plate has a yield strength of 420-460 MPa, a yield strength ratio of ≤0.75, an impact energy of not less than 190 J at -40°C, an elongation of ≥20%, and a cross-sectional shrinkage of ≥68%.
3. The anti-fatigue coated steel plate according to claim 1, characterized in that: The steel plate has a loading stress ratio of 0.1, a frequency of 90HZ, and a maximum stress of 0.75Rp 0.2 When the number of cycles reaches 10 7 The sample does not break, -20℃ CTOD δm>0.8mm.
4. A method for producing the anti-fatigue coated steel sheet according to any one of claims 1 to 3, characterized in that: It includes smelting, continuous casting, billet heating, controlled rolling and offline processing. The specific contents are as follows: Billet heating: The temperature of the cold billet into the furnace is controlled at 50-100℃, and multi-stage heating is adopted. The total time of 500-900℃ is controlled within 0.1-0.2min / mm, the total time of 1150-1180℃ is controlled within 0.1min / mm, and the total time of the soaking section 1120-1150℃ is controlled within 0.2-0.4min / mm; Controlled rolling: After the billet is taken out of the furnace, the temperature is raised to 950-1000℃ before rolling. The final rolling temperature is controlled above 900℃. The pass reduction in this stage is controlled at 20-30%, and the cooling rate after rolling is controlled at 3-7℃ / s. Off-line treatment: After the steel plate is off the line, the second stage precipitation phase and internal stress are regulated by thermal insulation treatment, and the thermal insulation regulation temperature is 320-390℃.
5. The method for producing an anti-fatigue coated steel sheet according to claim 4, characterized in that: The steel billet is made by converter smelting + continuous casting, and is pre-treated by rapid cooling when it is discharged. The surface temperature of the initial cooling is controlled at 815-890°C, and the cooling rate is controlled at 2-8°C / s. It is then subjected to low-temperature heating treatment at a treatment temperature of 220-370°C.
6. The method for producing an anti-fatigue coated steel sheet according to claim 4, characterized in that: The steel billet is smelted in a converter, the Ti element in the molten iron is controlled below 0.005%, and Si and Mn are used for deoxidation.
Citation Information
Patent Citations
High-anticorrosion low alloy steel suitable for high-temperature littoral environment
CN106929751A
X80-grade pipeline steel plate with seawater corrosion resistance and large deformation resistance and manufacturing method thereof
CN111961957A
High-performance corrosion-resistant fire-resistant steel with excellent toughness at low temperature of -80 DEG C and production method thereof
CN113604747A
Marine seawater corrosion fatigue resistant ultrahigh strength steel and manufacturing method thereof
CN114836694A
Structural steel excellent in fatigue crack propagation characteristics and coating durability, and method for producing the same
JP2020164951A