A method for suppressing tellurium-rich inclusion defects inside CZT crystals and improving their resistivity
By combining a dual-temperature zone horizontal annealing furnace with open-tube annealing, indium and tellurium are used as annealing sources to treat CZT crystals under nitrogen protection. This method solves the problem of tellurium-rich inclusion defects in CZT crystals, improves resistivity, and is applicable to the field of CZT crystal modification.
Patent Information
- Application Number
- CN202310306487.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Existing technologies are insufficient to effectively suppress tellurium-rich inclusion defects inside CZT crystals and improve their resistivity. Furthermore, existing methods are cumbersome and costly, making it difficult to meet the requirements of nuclear radiation detectors.
A method combining a dual-temperature zone horizontal annealing furnace with open-tube annealing is adopted, using indium and tellurium as annealing sources. Heat treatment is carried out in a nitrogen protective atmosphere, and tellurium-rich inclusions are removed through thermal migration mechanism. Indium and tellurium atoms are used to compensate for cadmium vacancies to improve resistivity.
It achieves a significant increase in the resistivity of CZT crystals while suppressing tellurium-rich inclusions. The operation is simple, low-cost, and has a short annealing cycle, making it suitable for the fabrication of nuclear radiation detectors.
Smart Images

Figure CN116334764B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of CZT crystal modification, and more specifically relates to a method for suppressing tellurium-rich inclusion defects inside CZT crystals and improving their resistivity. Background Technology
[0002] Cadmium zinc telluride (CZT) is a group II-VI compound semiconductor with a face-centered cubic structure, derived from cadmium telluride (CdTe) crystals. Due to its excellent photoelectric properties, CZT crystals are widely used in nuclear radiation detectors fabricated from it in fields such as astrophysics, security monitoring, environmental monitoring, medical imaging, and industrial control. However, CZT crystals have high growth temperatures, low thermal conductivity, and are prone to forming concave growth interfaces that are detrimental to crystal growth. This causes tellurium-rich melt at the growth interface front, deviating from the stoichiometric ratio, to be encapsulated by the concave growth interface, forming tellurium-rich inclusions and impairing the photoelectric properties of the CZT crystal. Furthermore, the high equilibrium vapor pressure of cadmium in CZT leads to its easy volatilization during crystal growth, resulting in a large number of cadmium vacancies and low resistivity in the grown state. Therefore, grown CZT crystals typically do not meet the requirements for fabricating nuclear radiation detectors and require post-processing.
[0003] Current processing methods have many drawbacks. For example, CN104532172A discloses a two-step heat treatment method for eliminating tellurium-rich precipitate defects in CZT materials. First, tellurium-rich CZT is heat-treated using a tellurium source to remove excess tellurium atoms from the crystal. Then, a cadmium source is used for heat treatment. However, this method is cumbersome, costly, and does not address the impact on the resistivity of the CZT crystal. CN102168313A discloses a vapor-phase annealing modification method for CZT crystals, which also employs a two-step annealing process. The first step uses non-metallic tellurium as the annealing source to improve the crystal's resistivity and energy resolution. The second step uses a cadmium-zinc alloy as the annealing source to eliminate inclusions and improve the carrier mobility-lifetime product. The sealing technology used in this method increases the consumption of quartz tubes, and the annealing time is over 2000 hours, resulting in excessively high time and economic costs and low practicality.
[0004] Therefore, how to provide a method to suppress tellurium-rich inclusion defects inside CZT crystals and improve their resistivity is a problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0005] In order to overcome the shortcomings and deficiencies of the prior art, the present invention provides a method for suppressing tellurium-rich inclusion defects inside CZT crystals and improving their resistivity. It has the characteristics of fewer operation steps, shorter annealing cycle, high efficiency and low cost, and can improve the resistivity of CZT crystals while suppressing tellurium-rich inclusion defects inside CZT crystals.
[0006] To achieve the above objectives, the present invention adopts the following technical solution:
[0007] A method for suppressing tellurium-rich inclusion defects and improving the resistivity of CZT crystals is proposed, which combines a dual-temperature zone horizontal annealing furnace with open-tube annealing heat treatment, using indium and tellurium as annealing sources and nitrogen as a protective atmosphere.
[0008] Preferably, the specific steps are as follows:
[0009] (1) Place the indium, tellurium and CZT crystals in quartz boats and put them in quartz tubes. Set the temperature control program through the temperature control operation interface, and then install the gas cylinder, inlet valve, quartz tube, outlet valve and vacuum pumping valve.
[0010] (2) Close the inlet valve, outlet valve and vacuum pump valve of the annealing furnace, turn on the mechanical pump to evacuate the environment inside the quartz tube, then turn on the vacuum pump valve and wait for the vacuum degree to be less than 1 Pa before closing the vacuum pump valve and turning off the mechanical pump; open the gas circuit in the order of main valve of gas cylinder, pressure dividing valve and pipeline switch, then open the inlet valve to introduce nitrogen into the quartz tube until the pressure inside the tube is equal to or slightly greater than atmospheric pressure, then close the inlet valve and stop the introduction of nitrogen.
[0011] (3) Repeat step (2) 2 to 5 times, then open the inlet valve and outlet valve to fill the quartz tube with nitrogen, turn on the temperature control system to run the annealing.
[0012] (4) The annealed CZT crystal is ground, mechanically polished, chemically polished, ultrasonically cleaned, and dried under vacuum.
[0013] Preferably, the dual-temperature zone horizontal annealing furnace consists of a temperature control system, a vacuum system, a gas flow control system, and a quartz tube furnace tube.
[0014] Preferably, the purity of both the quartz tube and the quartz boat is 4-5N.
[0015] Preferably, the purity of both the quartz tube and the quartz boat is 5N.
[0016] Preferably, the purity of both indium and tellurium is 6-7N.
[0017] Preferably, both indium and tellurium are particles with a particle size ≤ 5 mesh.
[0018] Preferably, the purity of both indium and tellurium is 7N.
[0019] Preferably, the nitrogen gas has a purity of 5N.
[0020] Preferably, the thickness of the CZT crystal is 1.0 to 5.0 mm.
[0021] Preferably, the nitrogen flow rate is 10 to 100 sccm.
[0022] Preferably, the temperature control program includes a heating rate, a cooling rate, a holding temperature, and a holding time; the heating rate and cooling rate are both 1 to 10 °C / min; the holding temperature in the low-temperature zone is 600 to 800 °C, the holding temperature in the high-temperature zone is 600 to 800 °C, and the holding time is 40 to 120 h.
[0023] Preferably, the heating rate and cooling rate are both 5-6℃ / min; the holding time is 60-70h.
[0024] Preferably, the quartz boats are placed in the following order: from the side closest to the annealing furnace inlet to the side closest to the outlet, there are quartz boats containing indium, tellurium, and CZT crystals, wherein the quartz boats containing indium and tellurium are located in the low-temperature zone, and the quartz boats containing CZT crystals are located in the high-temperature zone, and the distance between adjacent quartz boats is 5 to 15 cm.
[0025] Preferably, the distance between adjacent quartz boats is 10-15 cm.
[0026] Preferably, the air outlet and the low-temperature zone, and the high-temperature zone and the air inlet are separated by through-hole heat insulation plugs.
[0027] Preferably, the through-hole heat insulation plug is a ceramic alumina heat insulation plug or a quartz heat insulation plug.
[0028] Preferably, the through-hole heat insulation plug is a quartz heat insulation plug.
[0029] The mechanism of this invention is as follows:
[0030] The thermal migration mechanism is that when the annealing temperature is higher than the melting point of tellurium-rich inclusions in CZT, the molten tellurium-rich inclusions migrate from the interior of the crystal to the crystal surface through the action of the temperature gradient, and are then removed by grinding and polishing the annealed crystal.
[0031] Based on the self-compensation mechanism and the principle of electroneutrality, this invention utilizes indium and tellurium atmosphere annealing to allow indium and tellurium atoms to jointly compensate for cadmium vacancies in CZT crystals. Because the diffusion rate of indium atoms in CZT crystals is greater than that of tellurium atoms, a large number of cadmium vacancies are filled by indium atoms, forming shallow donor levels [In]. Cd ] + A small number of cadmium vacancies are compensated by tellurium atoms, generating deep donor levels [Te]. Cd ] 2+ The synergistic effect of indium and tellurium atoms significantly increases the resistivity of the annealed crystal.
[0032] As can be seen from the above technical solution, compared with the prior art, the present invention has the following beneficial effects:
[0033] This invention employs an annealing method combining a horizontal annealing furnace with independent dual-temperature zone control and open-tube annealing. This annealing method eliminates the need for tube welding, reduces operational steps, and allows for the reuse of quartz tubes. Furthermore, this invention uses a temperature higher than the melting point of tellurium-rich inclusions (which is less than 500°C) as the annealing temperature and indium and tellurium as the annealing source. This can suppress tellurium-rich inclusion defects within the crystal while improving the crystal resistivity, avoiding the cumbersome two-step annealing process. The annealing cycle is short, more efficient, and lower in cost, making it a more practical annealing method. Attached Figure Description
[0034] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.
[0035] Figure 1 This is a schematic diagram of the method described in this invention.
[0036] Figure 2 (a) and (b) are infrared transmission microscopy images of tellurium-rich inclusions in the CZT crystal of Example 1 before and after annealing, respectively.
[0037] Figure 3 (a) and (b) are infrared transmission micrographs of the tellurium-rich inclusions in the CZT crystal of Example 2 before and after annealing, respectively.
[0038] Figure 4 The images show the IV curves of the CZT crystal in Example 1 before annealing and after annealing in an indium and tellurium atmosphere for 60 hours.
[0039] Figure 5 The images show the IV curves of the CZT crystal before annealing and after annealing in an indium and tellurium atmosphere for 70 hours in Example 2. Detailed Implementation
[0040] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0041] Example 1
[0042] Preprocessing:
[0043] (1) Soak the quartz tube and quartz boat in aqua regia for 4 hours to remove the impurities attached to the quartz tube and quartz boat. Then rinse off the aqua regia remaining on the quartz tube and quartz boat with ultrapure water. Finally, purify the quartz tube and quartz boat with nitrogen gas at 800°C for 4 hours to remove moisture and impurities.
[0044] (2) Cut CZT crystals with a thickness of 2.2 mm from CZT ingots, then grind, mechanically polish, and chemically polish with 5% bromomethanol solution for 1 min. Then clean the chemically polished crystals with methanol, acetone and ethanol in sequence, then clean them with ultrapure water, and finally put them into a vacuum drying oven at 100℃ to dry for later use.
[0045] A method for suppressing tellurium-rich inclusion defects and improving the resistivity of CZT crystals includes the following steps:
[0046] (1) Using the pre-treated quartz tube, quartz boat and CZT crystal, indium, tellurium and CZT crystal are placed in the quartz boat and placed in the quartz tube. The temperature control program is set through the temperature control operation interface. Then the gas cylinder, gas inlet valve, quartz tube, gas outlet valve and vacuum pump valve are installed.
[0047] (2) Close the inlet valve, outlet valve and vacuum pump valve of the annealing furnace, turn on the mechanical pump to evacuate the environment inside the quartz tube, then turn on the vacuum pump valve and wait for the vacuum degree to be less than 1 Pa before closing the vacuum pump valve and turning off the mechanical pump; open the gas circuit in the order of main valve of gas cylinder, pressure dividing valve and pipeline switch, then open the inlet valve to introduce nitrogen into the quartz tube until the pressure inside the tube is equal to or slightly greater than atmospheric pressure, then close the inlet valve and stop the introduction of nitrogen.
[0048] (3) Repeat step (2) 3 times, then open the inlet valve and outlet valve to fill the quartz tube with nitrogen, turn on the temperature control system to run the annealing.
[0049] (4) Grind, mechanically polish, chemically polish, ultrasonically clean, and dry under vacuum after annealing CZT crystal;
[0050] The dual-temperature zone horizontal annealing furnace consists of a temperature control system, a vacuum system, a gas flow control system, and a quartz tube furnace tube.
[0051] The purity of both the quartz tube and the quartz boat is 5N;
[0052] The purity of both indium and tellurium is 7N;
[0053] Both indium and tellurium are particles with a particle size ≤ 5 mesh;
[0054] The nitrogen gas has a purity of 5N.
[0055] The thickness of the CZT crystal is 2.2 mm;
[0056] The nitrogen flow rate is 40 sccm;
[0057] The temperature control program includes heating rate, cooling rate, holding temperature, and holding time;
[0058] According to the principle of thermal migration, only when the annealing temperature is higher than the melting point of tellurium-rich inclusions can they melt and migrate from the interior of the crystal to the surface. Therefore, the annealing temperature generally needs to be higher than 500℃. Meanwhile, the fine structure phase diagram of the cadmium telluride homogeneous region at high temperatures shows that cadmium telluride undergoes a solid-state phase transition around 927℃, transforming from the β phase to the α phase of zinc sphalerite. The longer the two phases coexist, the greater the residual stress in the crystal, and the worse the crystal structure integrity. Based on this, the following settings were implemented: the heating and cooling rates are both 5℃ / min; the holding temperature in the low-temperature zone is 600℃, the holding temperature in the high-temperature zone is 700℃, and the holding time is 60h.
[0059] The quartz boats are placed in the following order: from the side closest to the annealing furnace inlet to the side closest to the outlet, there are quartz boats containing indium, tellurium, and CZT crystals, respectively. The quartz boats containing indium and tellurium are located in the low-temperature zone, while the quartz boats containing CZT crystals are located in the high-temperature zone. The distance between adjacent quartz boats is 15cm.
[0060] The air outlet and the low-temperature zone, as well as the high-temperature zone and the air inlet, are separated by through-hole heat insulation plugs.
[0061] The through-hole heat insulation plug is a ceramic alumina heat insulation plug.
[0062] The density of tellurium-rich inclusions within the obtained crystal was observed, and the IV curve of the crystal was tested, as shown below. Figure 2 and Figure 4 As shown, the tellurium-rich inclusion density decreased from 10 before annealing. 4 / cm 2 dropped to 10 3 / cm 2 The resistivity decreased from 1.767 × 10⁻⁶ before annealing. 7 The Ω·cm was increased to 2.546 × 10⁻⁶ after annealing. 10 Ω·cm.
[0063] Example 2
[0064] Preprocessing:
[0065] (1) Soak the quartz tube and quartz boat in aqua regia for 5 hours to remove the impurities attached to the quartz tube and quartz boat. Then rinse off the aqua regia remaining on the quartz tube and quartz boat with ultrapure water. Finally, purify the quartz tube and quartz boat with nitrogen gas at 800°C for 4 hours in an annealing furnace to remove moisture and impurities.
[0066] (2) Cut out CZT crystals with a thickness of 2.5 mm from CZT ingots, then grind, mechanically polish, and chemically polish with 5% bromomethanol solution for 90 seconds. Then clean the chemically polished crystals with methanol, acetone and ethanol in sequence, then clean them with ultrapure water, and finally put them into a vacuum drying oven at 100℃ to dry for later use.
[0067] A method for suppressing tellurium-rich inclusion defects and improving the resistivity of CZT crystals includes the following steps:
[0068] (1) Using the pre-treated quartz tube, quartz boat and CZT crystal, indium, tellurium and CZT crystal are placed in the quartz boat and placed in the quartz tube. The temperature control program is set through the temperature control operation interface. Then the gas cylinder, gas inlet valve, quartz tube, gas outlet valve and vacuum pump valve are installed.
[0069] (2) Close the inlet valve, outlet valve and vacuum pump valve of the annealing furnace, turn on the mechanical pump to evacuate the environment inside the quartz tube, then turn on the vacuum pump valve and wait for the vacuum degree to be less than 1 Pa before closing the vacuum pump valve and turning off the mechanical pump; open the gas circuit in the order of main valve of gas cylinder, pressure dividing valve and pipeline switch, then open the inlet valve to introduce nitrogen into the quartz tube until the pressure inside the tube is equal to or slightly greater than atmospheric pressure, then close the inlet valve and stop the introduction of nitrogen.
[0070] (3) Repeat step (2) 3 times, then open the inlet valve and outlet valve to fill the quartz tube with nitrogen, turn on the temperature control system to run the annealing.
[0071] (4) Grind, mechanically polish, chemically polish, ultrasonically clean, and dry under vacuum after annealing CZT crystal;
[0072] The dual-temperature zone horizontal annealing furnace consists of a temperature control system, a vacuum system, a gas flow control system, and a quartz tube furnace tube.
[0073] The purity of the quartz tube and quartz boat is the same as in Example 1;
[0074] The purity of both indium and tellurium is 7N;
[0075] Both indium and tellurium are particles with a particle size ≤ 5 mesh;
[0076] The nitrogen gas has a purity of 5N.
[0077] The thickness of the CZT crystal is 2.5 mm;
[0078] The nitrogen flow rate is 40 sccm;
[0079] The temperature control program includes heating rate, cooling rate, holding temperature, and holding time;
[0080] The heating rate and cooling rate are both 5℃ / min; the holding temperature in the low-temperature zone is 600℃, and the holding temperature in the high-temperature zone is 700℃; the holding time is 70h.
[0081] The quartz boats are placed in the following order: from the side closest to the annealing furnace inlet to the side closest to the outlet, there are quartz boats containing indium, tellurium, and CZT crystals, respectively. The quartz boats containing indium and tellurium are located in the low-temperature zone, while the quartz boats containing CZT crystals are located in the high-temperature zone. The distance between adjacent quartz boats is 10cm.
[0082] The air outlet and the low-temperature zone, as well as the high-temperature zone and the air inlet, are separated by through-hole heat insulation plugs.
[0083] The through-hole heat insulation plug is a quartz heat insulation plug.
[0084] The density of tellurium-rich inclusions within the obtained crystal was observed, and the IV curve of the crystal was tested, as shown below. Figure 3 and Figure 5 As shown, the tellurium-rich inclusion density decreased from 10 before annealing. 4 / cm 2 dropped to 10 3 / cm 2 The resistivity decreased from 2.172 × 10⁻⁶ before annealing. 7 The Ω·cm was increased to 5.685 × 10⁻⁶ after annealing. 10 Ω·cm.
[0085] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on its differences from other embodiments. Similar or identical parts between embodiments can be referred to interchangeably. The solutions disclosed in the embodiments are described simply because they correspond to the methods disclosed in the embodiments; relevant parts can be found in the method section.
[0086] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for suppressing tellurium-rich inclusion defects inside CZT crystals and improving their resistivity, characterized in that, A method combining a dual-temperature zone horizontal annealing furnace with open-tube annealing heat treatment is adopted, using indium and tellurium as annealing sources and nitrogen as a protective atmosphere. The specific steps are as follows: (1) Place the indium, tellurium and CZT crystals in quartz boats and place them in quartz tubes. Set the temperature control program through the temperature control operation interface, and then install the gas cylinder, inlet valve, quartz tube, outlet valve and vacuum pumping valve. (2) Close the inlet valve, outlet valve and vacuum pump valve of the annealing furnace, turn on the mechanical pump to evacuate the environment inside the quartz tube, then turn on the vacuum pump valve and wait for the vacuum degree to be less than 1 Pa before closing the vacuum pump valve and turning off the mechanical pump; open the gas circuit in the order of main valve of gas cylinder, pressure dividing valve and pipeline switch, then open the inlet valve and introduce nitrogen into the quartz tube until the pressure inside the tube is equal to or slightly greater than atmospheric pressure, then close the inlet valve and stop introducing nitrogen. (3) Repeat step (2) 2 to 5 times, then open the inlet valve and outlet valve to fill the quartz tube with nitrogen, turn on the temperature control system to run the annealing process; (4) Grind, mechanically polish, chemically polish, ultrasonically clean, and dry the annealed CZT crystal under vacuum. The temperature control program includes heating rate, cooling rate, holding temperature, and holding time; the heating rate and cooling rate are both 1~10℃ / min; the holding temperature of the low temperature zone is 600~800℃, the holding temperature of the high temperature zone is 600~800℃, and the holding temperature of the low temperature zone is lower than that of the high temperature zone. The heat preservation time is 40~120 hours; The quartz boats are placed in the following order: from the side closest to the annealing furnace inlet to the side closest to the outlet, there are quartz boats containing indium, tellurium, and CZT crystals, respectively. The quartz boats containing indium and tellurium are located in the low-temperature zone, while the quartz boats containing CZT crystals are located in the high-temperature zone. The distance between adjacent quartz boats is 5-15 cm.
2. The method for suppressing tellurium-rich inclusion defects and improving the resistivity of CZT crystals according to claim 1, characterized in that, The purity of both the quartz tube and the quartz boat is 4~5 N.
3. The method for suppressing tellurium-rich inclusion defects and improving the resistivity of CZT crystals according to claim 1, characterized in that, The purity of both indium and tellurium is 6~7 N; both indium and tellurium are particles with a particle size ≤ 5 mesh.
4. The method for suppressing tellurium-rich inclusion defects and improving the resistivity of CZT crystals according to claim 1, characterized in that, The nitrogen gas has a purity of 5N.
5. The method for suppressing tellurium-rich inclusion defects and improving the resistivity of CZT crystals according to claim 1, characterized in that, The thickness of the CZT crystal is 1.0~5.0 mm.
6. The method for suppressing tellurium-rich inclusion defects and improving the resistivity of CZT crystals according to claim 1, characterized in that, The nitrogen flow rate is 10~100 sccm.
7. The method for suppressing tellurium-rich inclusion defects and improving the resistivity of CZT crystals according to claim 1, characterized in that, The air outlet and the low-temperature zone, as well as the high-temperature zone and the air inlet, are separated by through-hole heat insulation plugs.
Citation Information
Patent Citations
Gas phase annealing modification method for tellurium / zinc / cadmium crystal
CN102168313A
Heat treatment method for eliminating tellurium-rich precipitate-phase defect in tellurium-zinc-cadmium material through two-step process
CN104532172A
CZT crystal, post-processing method of CZT crystal, CZT wafer, nuclear radiation detector and preparation methods of CT wafer and nuclear radiation detector
CN113151901A