A lightweight flexible electromagnetic shielding fiber membrane material and its preparation method and application

Through the combination of thermal imidation and hot pressing, combined with formaldehyde-free wet electroless plating solution and corrosion-resistant active agent, the fiber membrane has solved the problems of short service life and low shielding efficiency in special environments, and achieved high efficiency and corrosion resistance The electromagnetic shielding performance is suitable for a variety of application scenarios.

CN116334916BActive Publication Date: 2024-12-03JIANGNAN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310103721.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-10
Publication Date
2024-12-03
Estimated Expiration
2043-02-10

AI Technical Summary

Technical Problem

The prior art has difficulty in preparing electromagnetic shielding materials, especially in chemical plating without palladium activation. The fiber membrane obtained by electrospinning has a short service life, poor flexibility, corrosion resistance, and low shielding efficiency under special environments. , the problem of narrow bandwidth.

Method used

The polyamic acid fiber membrane is treated by combining thermal imidation and hot pressing. The specific crude liquid and metal salt are used as activators to metallize through a formaldehyde-free wet electroless plating solution to combine with corrosion-resistant surfaces. Active agents form efficient and controllable metal coatings to improve bonding and corrosion resistance between fibers.

Benefits of technology

It has achieved the preparation of high-efficiency metallized polyimide fiber membranes, with excellent electromagnetic shielding performance, long service life, strong corrosion resistance, and wide frequency bandwidth. It is suitable for special environments, especially in the fields of aerospace and military equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116334916B_ABST
    Figure CN116334916B_ABST
Patent Text Reader

Abstract

The present invention discloses a light and flexible electromagnetic shielding fiber membrane material and a preparation method and application thereof, and belongs to the technical field of electromagnetic shielding materials. The preparation of the light and flexible electromagnetic shielding fiber membrane material of the present invention is to treat the polyamic acid salt fiber membrane in a combination of thermal imidization and hot pressing to reduce the space between fibers, and then use a roughening liquid to achieve surface roughening of the polymer material, while using a specific metal salt as an activator of a wet-chemical plating solution, and using a formaldehyde-free plating solution in a "green and environmentally friendly" manner to achieve efficient and controllable construction of metallized polymer materials, and finally surface treatment is performed on it through surface anticorrosion to enhance its corrosion resistance. The material has good flexibility and strong electromagnetic shielding performance, and is expected to be used in the fields of aerospace, military equipment, microelectronic equipment, and civilian electrical appliances.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a light flexible electromagnetic shielding fiber membrane material and a preparation method and application thereof, belonging to the technical field of electromagnetic shielding materials. Background Art

[0002] Electromagnetic shielding materials, as a functional protective material that effectively isolates incident electromagnetic waves by means of reflection loss outside the material and absorption loss inside the material, have been widely used in the field of electromagnetic protection. At the same time, the miniaturization and high integration of electronic components have also made electromagnetic leakage and interference problems in electrical equipment increasingly prominent. Under some special extreme conditions such as extremely cold, hot or humid environments, the high and low temperature resistance and corrosion resistance of conventional shielding materials are generally very poor, and the shielding performance is greatly attenuated, which cannot meet the actual use needs.

[0003] Therefore, people have put forward higher performance requirements for high-performance electromagnetic shielding materials, requiring them to have excellent high and low temperature resistance and corrosion resistance in special environments in addition to the characteristics of thinness, lightness, width, and strength. Polyimide fiber materials have attracted widespread attention for their excellent high and low temperature resistance, excellent flexibility, and high strength. However, polyimide fibers have no obvious shielding effect on incident electromagnetic waves because they are non-conductive and non-magnetic.

[0004] Therefore, in order to obtain high-performance electromagnetic shielding materials, it is usually necessary to give polyimide fibers excellent electrical conductivity and magnetic conductivity. Generally speaking, surface metallization of polymer matrix is ​​a common method to obtain excellent electrical conductivity and magnetic conductivity.

[0005] The surface metallization methods of polymer materials can be divided into two categories: the first category is the dry method, which mainly includes physical vapor deposition and chemical vapor deposition. Physical vapor deposition can be divided into vacuum evaporation and magnetron sputtering. The vacuum evaporation method can form a metal coating on the surface of the polymer material in an extremely short time, but the bonding force between the metal layer and the polymer substrate is poor, and the vacuum evaporation method also limits the use of metal materials with a low melting point such as aluminum, which greatly limits its application. The magnetron sputtering method uses high-energy ions to bombard the metal target material so that the target atoms obtain enough energy to sputter and deposit on the surface of the polymer material; compared with the vacuum evaporation method, the magnetron sputtering method can improve the bonding force between the metal coating and the polymer substrate, and is suitable for a variety of metal materials such as aluminum, silver, and nickel, but there are restrictions on the use of metallization on the inner surface of three-dimensional materials with spatial structures (such as fiber non-woven fabrics), and the equipment cost is relatively high. Chemical vapor deposition uses reactive gases to react chemically on the surface of the substrate to achieve metal atom deposition. The resulting metal film is uniform and dense, and its bonding force with the substrate is also strong; however, the reaction temperature of this method is usually very high (900-2000°C), which can easily lead to deformation and structural changes in the substrate, and is not suitable for polymer materials. The second type is the wet method, which mainly includes electroplating, redox method and chemical plating. Electroplating uses electrolysis to achieve surface metallization of polymer materials. This method has uniform crystallization and low roughness, and has strong bonding force with the substrate, without peeling, pinholes, burrs and other phenomena; however, this method requires the use of chromium / nickel metal derivatives that are harmful to the environment, and the polymer materials that are currently most used in electroplating are mainly ABS and polypropylene (PP), followed by polysulfone (PSF), polycarbonate (PC) and polytetrafluoroethylene (PTFE), but it is difficult to apply. The chemical reduction method is to form a chelate between metal salts and polymer molecules, introduce metal ions into the surface of polymer materials, and then use a reducing agent to reduce the metal ions, thereby forming a metal layer on the surface of the substrate. Unlike chemical reduction, chemical plating utilizes a "roughening-activation" process to form active catalytic centers on the surface of polymer materials that induce subsequent metal ion reduction reactions, thereby achieving uniform loading of metal coatings on the surface of substrate materials. This method is simple to operate and has strong all-over plating ability. It is suitable for plating materials with complex shapes and inner holes or cavities. The coating is uniform and dense, with low porosity and strong applicability. It can deposit coatings on metal, non-metal, and polymer substrates.

[0006] Conventional chemical plating pretreatment, especially the roughening process, is the key to affecting the bonding strength between the metal layer and the substrate. However, most polymer materials are difficult to effectively roughen due to their surface inertia. On the other hand, activation, as a key step in chemical plating pretreatment, directly affects the uniformity and selectivity of the catalyst's adhesion on the surface of the plated part, and determines the continuity of the coating itself. Currently, palladium activation is the main method, which is costly and polluting.

[0007] Although researchers have developed a non-activation process to achieve one-step chemical copper plating on the surface of nylon fibers, the lack of activation centers will significantly reduce the rate of copper deposition, which is not conducive to its promotion and application on production lines. Therefore, the research focus of palladium-free activation will shift to precious metals such as gold, silver, and platinum that also have catalytic activity; among them, chemical copper plating is easier, and silver activation can complete the catalysis; but chemical plating of cobalt and nickel is more difficult, and platinum with strong catalytic properties must be used.

[0008] In addition, nickel, as a high magnetic permeability metal, has strong ability to absorb and scatter electron vectors of radiation and large attenuation of magnetic vectors, and has been widely used in the field of electromagnetic shielding. However, to date, there has been no report on the research of efficient chemical nickel plating on the surface of polymer materials without palladium activation and its electromagnetic shielding performance. Summary of the invention

[0009] [Technical issues]

[0010] In the process of preparing electromagnetic shielding materials by chemical plating in the prior art, there are problems such as great difficulty in chemical plating, especially chemical plating without palladium activation; and for the fiber membrane obtained by electrospinning, due to its internal fluffy structure, there is no cross-linking between fibers, resulting in poor mechanical properties, and the resistance of the fiber membrane after chemical metallization is large.

[0011] Therefore, how to achieve a strong bonding roughened surface, efficient metallization and anti-corrosion treatment for polymer fiber materials to obtain lightweight flexible electromagnetic protection materials with long service life, corrosion resistance, high shielding efficiency and wide bandwidth has become a key issue and challenge that needs to be solved urgently.

[0012] [Technical solution]

[0013] In order to solve the above problems, the present invention provides a method for preparing a metallized polyimide fiber electromagnetic shielding material that is resistant to high and low temperatures and corrosion, with the aim of overcoming the bottleneck problems of short service life, poor flexibility, corrosion resistance, low shielding effectiveness, and narrow frequency bandwidth of traditional electromagnetic shielding materials under special environments. The present invention treats the polyamic acid salt fiber membrane by combining thermal imidization and hot pressing to reduce the space between fibers, and then uses a specific roughening liquid to achieve surface roughening of the polymer material. At the same time, a specific metal salt is used as an activator for a wet-chemical plating solution, and a formaldehyde-free plating solution is used in a "green and environmentally friendly" manner to achieve efficient and controllable construction of the metallized polymer material. Finally, a specific surfactant is used to perform surface treatment on the material to enhance its corrosion resistance.

[0014] Specifically: (1) The present invention uses a combination of thermal imidization and hot pressing to hot press the polyamic acid salt fiber membrane, so that the fibers are in contact with each other, laying the foundation for the metallized fiber conductive path; (2) The specific roughening liquid can form a polymer coating with very strong adhesion on the surface of the polymer material through a polymerization reaction in an aqueous solution. At the same time, the polymer contains a large number of functionalized functional groups, which have strong complexing and reducing abilities for metal ions, and can in situ reduce specific non-palladium noble metal ions to metal elements, and use them as catalytic centers to efficiently promote the reduction of metal ions such as copper / nickel / silver in the chemical plating solution, thereby depositing metal copper / nickel / silver on the surface, providing a "chemical" anchor point for subsequent chemical plating. The bonding force between the subsequent metal coating and the polymer material is improved, and the stability and service life of the material are extended; (3) The present invention adopts a palladium-free and fluorine-free activation process and a formaldehyde-free plating solution system, which provides a new path for the efficient, green and environmentally friendly preparation of material surface metallization; (4) Nickel, as a high magnetic permeability conductive metal, has electromagnetic shielding properties extending to the low frequency band. The rational construction of the multi-level microstructure inside the metallized polyimide fiber will provide new possibilities for enhancing its electromagnetic interference shielding effectiveness and widening the bandwidth; (5) The use of corrosion-resistant surfactants can form a self-assembled molecular film on the surface of face-centered cubic metals (silver, copper or nickel), which has a barrier effect on water and oxygen molecules, and contributes to improving the corrosion resistance of the metal coating.

[0015] The object of the present invention is to provide a method for preparing a lightweight flexible electromagnetic shielding fiber membrane material, the method comprising the following steps:

[0016] (1) Preparation of polyamic acid salt spinning solution

[0017] Dissolve the diamine and dibasic anhydride monomers in an organic solvent, stir to react with polymerization, then add an organic base, stir thoroughly, transfer to an acetone solvent to complete solvent exchange, and remove the supernatant; then take the precipitate and place it in a vacuum oven to dry to obtain polyamic acid salt, then place the polyamic acid salt in a water-alcohol mixed solution to fully dissolve it to obtain a polyamic acid salt spinning solution;

[0018] (2) Preparation of polyimide fiber membrane

[0019] The polyamic acid salt spinning solution obtained in step (1) is processed by an electrostatic spinning process to obtain a polyamic acid fiber membrane, and the polyamic acid fiber membrane is placed in an inert gas atmosphere for thermal imidization treatment to obtain a polyimide fiber membrane material;

[0020] (3) Preparation of metallized polyimide fiber membrane

[0021] The polyimide fiber membrane obtained in step (2) is first roughened in a roughening solution; then the roughened polyimide fiber membrane is immersed in an activation solution for treatment; finally, the activated polyimide fiber membrane is immersed in a plating solution for plating treatment, washed and dried to obtain a metallized polyimide fiber membrane material; the solute in the activation solution is chloroplatinic acid, the concentration is 0.1-20 g / L, the activation treatment time is 30 min-120 min; the plating treatment time is 10-60 min, and the temperature is 10-30° C.;

[0022] (4) Corrosion resistance treatment

[0023] The metallized polyimide fiber membrane material prepared in step (3) is immersed in a metal anti-corrosion treatment liquid, and then vacuum dried after the treatment.

[0024] In one embodiment, the dianhydride monomer in step (1) is one or more of pyromellitic dianhydride (PMDA), biphenyltetracarboxylic dianhydride (BPDA), 3,3',4,4-benzophenonetetracarboxylic dianhydride (BTDA), and 4,4'-oxydiphthalic anhydride (ODPA); the diamine monomer is one or more of 4,4'-diaminodiphenyl ether (ODA), p-phenylenediamine (PDA), and 4,4"-diaminoterphenyl (DAT).

[0025] In one embodiment, the organic solvent in step (1) is one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), tetrahydrofuran (THF), and N-methylpyrrolidone (NMP).

[0026] In one embodiment, the polymerization reaction in step (1) is carried out at a temperature of 0 to 10° C. and for a time of 2 to 5 hours.

[0027] In one embodiment, the organic base in step (1) is one or more of triethylamine (TEA), quinoline (QL), and N,N-dimethylethanolamine (DMEA); and the stirring time after adding the organic base is 1 to 3 hours.

[0028] In one embodiment, the time for the solvent exchange in step (1) is 20 to 60 minutes.

[0029] In one embodiment, the vacuum drying temperature in step (1) is 40-70°C.

[0030] In one embodiment, the mass ratio of alcohol in the water-alcohol mixed solution in step (1) is 40-90%, wherein the alcohol solvent is any one of ethanol, methanol and propanol; and the solid content of the polyamic acid salt spinning solution is 5-12%.

[0031] In one embodiment, the positive electrode voltage of the polyamic acid salt spinning solution electrospinning in step (2) is 17-30 kV; the negative electrode voltage is 0.5-2 kV; the propulsion speed is 0.1-0.2 mL / min, and the distance between the needle and the receiver is 10-30 cm.

[0032] In one embodiment, the temperature of the thermal imidization treatment in step (2) is 300-400° C., and the time is 0.5-2 h; and the inert protective gas is one or more of nitrogen, argon, and helium.

[0033] In one embodiment, the thermal imidization treatment in step (2) further comprises using a quartz plate to clamp the polyamic acid salt fiber membrane for thermal imidization treatment.

[0034] In one embodiment, the solute in the roughening solution of step (3) is one or more of dopamine, citric acid, polyphenolamine, and tannic acid; the concentration is 2 to 6 g / L, and the treatment time is 1 h to 24 h.

[0035] In one embodiment, the vacuum drying time of the roughened polyimide fiber membrane in step (3) is 1 to 2 hours, and the drying temperature is 40 to 60°C.

[0036] In one embodiment, the vacuum drying time of the activated metallized polyimide fiber membrane in step (3) is 1 to 2 hours, and the drying temperature is 40 to 60°C.

[0037] In one embodiment, the plating solution in step (3) includes a metal salt, a complexing agent, a reducing agent, and a pH adjusting agent.

[0038] In one embodiment, the metal salt is one or more of nickel sulfate, nickel chloride, and nickel nitrate, and the concentration is 8 to 80 g / L.

[0039] In one embodiment, the complexing agent is one or more of lactic acid, sodium citrate, tartaric acid, acetic acid, sodium acetate, malic acid, thiourea, and ammonium chloride, and the concentration is 5 to 20 g / L.

[0040] In one embodiment, the reducing agent is one or more of dimethylamine borane and sodium hypophosphite, and the concentration is 1 to 10 g / L.

[0041] In one embodiment, the pH adjuster is one or more of ammonia water, sodium hydroxide, potassium hydroxide, hydrochloric acid, and sulfuric acid, and the pH is adjusted to 4.8-10.

[0042] In one embodiment, the plating treatment time in step (3) is 10 to 60 minutes and the temperature is 10 to 30°C.

[0043] In one embodiment, the vacuum drying time after the polyimide fiber membrane is plated in step (3) is 1 to 2 hours, and the drying temperature is 40 to 60°C.

[0044] In one embodiment, the solute of the anti-corrosion treatment liquid in step (4) is one or more of octadecyl mercaptan, epoxytrimethoxysilane coupling agent, and γ-aminopropyltriethoxysilane, and the solvent is one or more of ethanol, methanol, propanol acetic acid, and formic acid; and the immersion time is 10 to 30 minutes.

[0045] In one embodiment, the vacuum drying time of the metallized polyimide fiber membrane after anti-corrosion treatment in step (4) is 1 to 2 hours, and the drying temperature is 20 to 50°C.

[0046] The second object of the present invention is to provide a lightweight and flexible electromagnetic shielding fiber membrane material prepared by the above-mentioned method.

[0047] The third object of the present invention is to provide an application of the above-mentioned lightweight flexible electromagnetic shielding fiber membrane material in the field of electromagnetic protection of aerospace devices, military equipment or precision electronic instruments.

[0048] [Beneficial Effects]

[0049] (1) The preparation method of the present invention is simple to operate and is green and environmentally friendly. The present invention synthesizes water-based polyamic acid salt and dissolves the polyamic acid salt in a water-alcohol solution, and uses electrospinning technology to prepare polyimide micron fibers. Then, the polyimide fibers are roughened, activated, plated and subjected to corrosion resistance treatment to obtain a metallized corrosion-resistant polyimide fiber membrane material with a skin-core structure.

[0050] Under the roughening effect, active functional groups such as amino, carboxyl, and phenolic hydroxyl groups were successfully loaded on the surface of polyimide fibers. Based on the adsorption and reducibility of these functional groups to metal ions, Pt + 、Ag + , Cu 2+ The metal ions are in situ reduced and successfully loaded on the surface of the polyimide fiber. These catalytically active metal particles can serve as active centers during the plating process to achieve palladium-free and fluorine-free activation, which is green and environmentally friendly, greatly increasing the uniformity of plating and the efficiency of plating. The fiber membrane material obtained by electrospinning has a porous structure, which causes electromagnetic waves to be scattered / reflected multiple times inside the material, greatly improving the electromagnetic shielding performance; in addition, the polyimide fiber membrane obtained by electrospinning has high mechanical strength and flexibility, so that the metallized polyimide fiber membrane material obtained by the present invention has a wide range of application prospects.

[0051] (2) The present invention is based on the principle that the incident electromagnetic wave undergoes multiple scattering / reflection loss attenuation inside the material, obtains a lightweight and porous polyimide fiber membrane material through electrostatic spinning technology, and successfully loads metal nickel on the polyimide fiber through a chemical plating process. The high electrical conductivity and high magnetic permeability of nickel enable the electromagnetic wave to be effectively reflected and absorbed on the surface of the material. In addition, the porous structure inside the material enables the electromagnetic wave to undergo multiple scattering / reflection inside the material, and the electromagnetic shielding effectiveness (>20dB) can cover the entire X-band.

[0052] At the same time, the internal porous structure obtained by electrospinning and the low density of the polymer itself make the material have an extremely low density. In addition, applying pressure to the polyamic acid salt film material during the thermal imidization process can greatly reduce the distance between the fibers, so that a tighter conductive path can be formed between the fibers during the subsequent chemical plating process, which greatly improves the conductivity of the film material, thereby making the film show higher electromagnetic shielding performance in a thinner case. For example, when the thickness of the metallized polyimide film material without heat pressing is 238μm, the density is only 0.174g / cm 3 , the conductivity is 57S / cm, and the electromagnetic shielding effectiveness can reach 31dB in the entire X-band; for the polyamic acid salt fiber membrane of the same thickness, the density is increased to 0.905g / cm after chemical nickel plating after hot pressing. 3 The conductivity is increased to 953S / cm, the thickness is reduced to 57μm, and the electromagnetic shielding effectiveness can be increased to 69dB in the entire X-band, far exceeding similar materials.

[0053] (3) The preparation process of the present invention is simple and easy to operate, and is expected to be applied to fields that require electromagnetic shielding, such as aerospace, military equipment, microelectronic equipment, and civilian electrical appliances. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 Optical images of the polyimide fiber membrane (a) and the metallized polyimide fiber membrane (b, c) in Example 1 of the present invention;

[0055] Figure 2 is a scanning electron microscope image of the polyimide fiber (a) and the metallized polyimide fiber (b) in Example 1 of the present invention;

[0056] Figure 3 The electromagnetic shielding effectiveness graph (a) and the conductivity graph (b) of the metallized polyimide fiber membrane with and without heat pressing treatment in Examples 1 and 2 of the present invention are shown;

[0057] Figure 4 The electromagnetic shielding effectiveness (a) and electrical conductivity (b) of the material formed at different plating times according to Example 3 of the present invention are shown;

[0058] Figure 5 This is a comparison diagram of the electromagnetic shielding effectiveness of Ni@PI-HP prepared in Example 2 of the present invention before and after treatment at 350°C for 1h in an air atmosphere;

[0059] Figure 6 This is a comparison diagram of the electromagnetic shielding effectiveness of Ni@PI-HP prepared in Example 2 of the present invention before and after being immersed in liquid nitrogen for 24 hours;

[0060] Figure 7 This is a comparison diagram of the electromagnetic shielding effectiveness of Ni@PI-HP prepared in Example 2 of the present invention before and after 10,000 bendings;

[0061] Figure 8 This is a comparison chart of the electromagnetic shielding effectiveness of Ni@PI-HP prepared in Example 2 of the present invention before and after being treated in neutral salt spray for 100h and 200h. DETAILED DESCRIPTION

[0062] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0063] Characterization and performance testing:

[0064] 1. Scanning electron microscope image determination method: The scanning electron microscope image of the composite fiber membrane material was taken using a JSM 6490LV field emission electron microscope from Japan's JEOL Company.

[0065] 2. Electromagnetic shielding effectiveness determination method: The S parameters of the composite film were measured by the waveguide method in the frequency range of 8.2 to 12.4 GHz using an Agilent E5063A vector network analyzer.

[0066] 3. Conductivity determination method: The conductivity of the composite material sample was determined using Suzhou Jingge Electronics ST2263 dual-electric digital four-probe tester using a standard four-point contact method.

[0067] 4. Neutral salt spray test: Referring to the national standard GB / T5170.2-96, the prepared composite material is placed on the rack of the salt spray test machine, the laboratory temperature controller is set to 35°C, the pressure barrel temperature controller is set to 40-50°C, and the salt spray time is set to 100h and 200h.

[0068] Example 1

[0069] A method for preparing a lightweight flexible electromagnetic shielding fiber membrane material, the method comprising the following steps:

[0070] (1) Preparation of polyimide fiber membrane

[0071] Preparation of polyamic acid salt powder: 96.6 g N, N-dimethylformamide (DMF), 8 g 4, 4'-diaminodiphenyl ether (ODA) and 8.9 g pyromellitic anhydride (PMDA) were added to a 250 mL three-necked flask in sequence, and mechanical stirring was continued for 2.5 h in a 0-10 ° C water bath, followed by adding 100 g of DMF, stirring was continued for 1.5 h, and then 5.2 ml N, N-

[0072] dimethylethanolamine (DMEA), stirring continuously for 3 hours to carry out polymerization reaction; finally, the polymer after the reaction was transferred to acetone and stirred continuously for a period of time and then allowed to stand, and the supernatant was poured out after complete sedimentation, and the above steps were repeated 3 times, and the precipitate was placed in a vacuum oven and vacuum dried at 50°C for 8 hours to obtain polyamic acid salt powder;

[0073] Preparation of polyamic acid salt spinning solution: Weigh 5 g of the polyamic acid salt powder prepared above and add it to 45 g of a 50% water-ethanol mixture, and continue stirring for 24 hours to fully dissolve it to obtain a polyamic acid salt spinning solution (solid content of 10.0%);

[0074] Preparation of polyimide fiber membrane: 30 mL of polyamic acid salt spinning solution was electrospun at a propulsion speed of 0.1 mL / min, a positive voltage of 24 kV, a negative voltage of 0.5 kV, and a receiving distance of 20 cm. After the electrospinning was completed, the fiber membrane was peeled off from the receiving roller to obtain a polyamic acid salt fiber membrane; the polyamic acid salt fiber membrane was then placed in a tubular furnace (argon atmosphere) at 350°C for 1 hour, cooled to room temperature and then taken out to obtain a polyimide fiber membrane; named PI;

[0075] (2) Preparation of metallized polyimide fiber membrane

[0076] Roughening: The polyimide fiber membrane prepared above was placed in a tris solution with a pH of 8.5, and ultrasonicated for 2 minutes to completely infiltrate the polyimide fiber membrane, and then 1.5 g of dopamine was added, and the mixture was stirred for 24 hours under magnetic stirring; after the completion, the polyimide fiber membrane was washed with ultrapure water for 2 to 3 times, ultrasonically cleaned for 1 minute, and then washed once with anhydrous ethanol, and finally placed in a vacuum oven at 50°C for vacuum drying for 2 hours to obtain a roughened polyimide fiber membrane;

[0077] Activation: The roughened polyimide fiber membrane was placed in 150 mL of 1.5 g / L chloroplatinic acid solution, and magnetic stirring was continued for 0.5 h. After being fully washed with ultrapure water and anhydrous ethanol, the membrane was placed in a vacuum oven at 50° C. and vacuum dried for 2 h to obtain an activated polyimide fiber membrane.

[0078] Plating: The activated polyimide fiber membrane was placed in 150 mL of plating solution and plated at 25°C for 30 min. After plating, the membrane was taken out and washed thoroughly with ultrapure water and anhydrous ethanol. Finally, the membrane was placed in a vacuum oven at 50°C and dried for 2 h to obtain a metallized polyimide fiber membrane, named Ni@PI.

[0079] The concentration of nickel sulfate hexahydrate in the plating solution is 80 g / L, the concentration of sodium citrate dihydrate is 40 g / L, the concentration of lactic acid is 20 g / L, and the concentration of dimethylamine borane is 10 g / L.

[0080] Anti-corrosion treatment: The metallized polyimide fiber membrane prepared above was immersed in a solution containing 0.0015 mol of octadecyl mercaptan, 144 mL of ethanol, and 6 mL of acetic acid. After soaking for 30 minutes, it was taken out and dried in a vacuum oven at 40°C for 1 hour to obtain a metallized polyimide fiber membrane with anti-corrosion properties.

[0081] Example 2

[0082] A method for preparing a lightweight flexible electromagnetic shielding fiber membrane material, the method comprising the following steps:

[0083] (1) Preparation of polyimide fiber membrane

[0084] Preparation of polyamic acid salt fiber membrane: Take 30 mL of the polyamic acid salt spinning solution in Example (1), and perform electrospinning at a propulsion speed of 0.1 mL / min, a positive electrode voltage of 24 kV, a negative electrode voltage of 0.5 kV, and a receiving distance of 20 cm. After the spinning, remove the fiber membrane from the receiving roller to obtain the polyamic acid salt fiber membrane;

[0085] Preparation of polyimide fiber membrane: The polyamic acid salt fiber membrane was clamped by a quartz plate and placed in a tube furnace (argon atmosphere) at 350°C for 1 hour, and then taken out after cooling to room temperature to obtain a hot-pressed polyimide fiber membrane; named PI-HP;

[0086] (2) Preparation of metallized polyimide fiber membrane

[0087] Roughening: The hot-pressed polyimide fiber membrane was placed in a tris solution with a pH value of 8.5, and ultrasonicated for 2 minutes to completely infiltrate the fiber membrane, and 1.5 g of dopamine was added, and the mixture was stirred for 24 hours under magnetic stirring. After the mixture was finished, the polyimide fiber membrane was washed with ultrapure water for 2 to 3 times, ultrasonically cleaned for 1 minute, and then washed once with anhydrous ethanol, and then placed in a vacuum oven at 50°C for vacuum drying for 2 hours to obtain a roughened polyimide fiber membrane.

[0088] Activation: The roughened polyimide fiber membrane was placed in 150 mL of 1.5 g / L chloroplatinic acid solution and continuously stirred with magnetic stirring for 0.5 h. After being taken out, it was thoroughly washed with ultrapure water and anhydrous ethanol, and then placed in a vacuum oven at 50 ° C for 2 h to obtain an activated polyimide fiber membrane;

[0089] Plating: The activated polyimide fiber membrane was placed in 150 mL of plating solution and plated at 25°C for 30 min. After plating, the membrane was taken out and washed thoroughly with ultrapure water and anhydrous ethanol. Finally, the membrane was placed in a vacuum oven at 50°C for 2 h to obtain a metallized polyimide fiber membrane, named Ni@PI-HP.

[0090] The concentration of nickel sulfate hexahydrate, sodium citrate dihydrate, lactic acid, and dimethylamine borane in the plating solution is 80 g / L, 40 g / L, 20 g / L, and 10 g / L.

[0091] Anti-corrosion treatment: The prepared metallized polyimide fiber membrane (Ni@PI-HP) was immersed in a solution containing 0.0015 mol of octadecyl mercaptan, 144 mL of ethanol, and 6 mL of acetic acid. After soaking for 30 min, it was taken out and dried in a vacuum oven at 40 °C for 1 h; thus, a corrosion-resistant metallized polyimide fiber membrane was obtained.

[0092] Example 3

[0093] The plating time in step (2) of Example 2 was adjusted to 20 min, 25 min and 35 min respectively; other conditions were the same as those in Example 2, and a corrosion-resistant metallized polyimide fiber membrane was obtained.

[0094] Example 4

[0095] The concentration of the chloroplatinic acid solution in step (2) of Example 2 was adjusted to 0.1 g / L, the plating time was 60 min, and the other conditions were the same as in Example 2. Due to the decrease in the concentration of chloroplatinic acid, the reaction rate was relatively reduced, and after extending the plating time, a corrosion-resistant metallized polyimide fiber membrane was obtained.

[0096] Example 5

[0097] The concentration of the chloroplatinic acid solution in step (2) of Example 2 is adjusted to 20 g / L, the plating time is 10 min, and the other conditions are the same as those in Example 2. Due to the increase in the concentration of chloroplatinic acid, the reaction rate is improved, and a corrosion-resistant metallized polyimide fiber membrane can be obtained in a short time.

[0098] Example 6

[0099] Plating: Place the activated polyimide fiber membrane in Example 2 in 150 mL of plating solution, in which the concentration of nickel sulfate hexahydrate, sodium acetate, acetic acid, thiourea and sodium hypophosphite is 27 g / L, 20 g / L, 16 g / L, 1 mg / L and 32 g / L respectively; plate at 85°C for 10 min, wash twice with ultrapure water and anhydrous ethanol respectively after plating, and finally place in a vacuum oven at 50°C for vacuum drying for 2 h to obtain a metallized polyimide fiber membrane; treat in the anti-corrosion solution in Example 1 to obtain an anti-corrosion treated metallized polyimide fiber membrane.

[0100] Example 7

[0101] Plating: Place the activated polyimide fiber membrane in Example 1 in 150 mL of plating solution, in which the concentration of nickel sulfate hexahydrate is 30 g / L, the concentration of sodium citrate is 10 g / L, the concentration of ammonium chloride is 30 g / L, and the concentration of sodium hypophosphite is 30 g / L. Plating is performed at 45°C for 2 hours. After plating, the membrane is taken out and washed twice with ultrapure water and anhydrous ethanol respectively, and finally placed in a vacuum oven at 50°C for 2 hours to obtain a metallized polyimide fiber membrane. After treatment in the anticorrosive solution in Example 1, a corrosion-resistant metallized polyimide fiber membrane is obtained.

[0102] Comparative Example 1

[0103] The concentration of the chloroplatinic acid solution in step (2) of Example 2 was adjusted to 0.05 g / L of chloroplatinic acid, and the other conditions were the same as those in Example 2 to obtain a metallized polyimide fiber membrane.

[0104] As the concentration of chloroplatinic acid decreases, the reaction rate decreases and the uniformity of the obtained metallized polyimide fiber membrane is poor.

[0105] Comparative Example 2

[0106] The concentration of the chloroplatinic acid solution in step (2) in Example 2 is adjusted to 40 g / L of chloroplatinic acid solution, and other conditions are the same as those in Example 2. Due to the high concentration of chloroplatinic acid, the reaction rate is too fast, causing the plating solution to lose stability in a short period of time, and the nickel plating effect on the polyimide fiber film is uneven.

[0107] Comparative Example 3

[0108] The only difference from Example 2 is that the activation step in step (2) is omitted, and the rest is the same as Example 2.

[0109] What is obtained is a non-metallized polyimide fiber membrane. Due to the absence of active sites, no metal is deposited on the surface of the metal fiber during the plating process, and the chemical plating process cannot be carried out.

[0110] Test analysis

[0111] 1. Determination of flexibility of polyimide fiber membrane materials and metallized polyimide fiber membranes

[0112] Figure 1 The following are photos of the polyimide fiber membrane material (PI) and the metallized polyimide fiber membrane material (Ni@PI) in Example 1, wherein Figure 1 (a) is a physical photo of PI, Figure 1 (b) and (c) are actual photos of Ni@PI.

[0113] from Figure 1 It can be seen that the polyimide fiber membrane material obtained by electrospinning has very good softness and scalability. The polyimide fiber membrane material after chemical nickel plating can be seen from the figure that it exhibits excellent uniformity on a macro scale. Even if the surface of the polyimide fiber is metallized, it still has excellent softness and can be folded into the shape of a "thousand paper cranes".

[0114] 2. Structural characterization of metallized polyimide fiber membrane materials

[0115] Figure 2 The scanning electron microscope photos of polyimide fiber membrane material and metallized polyimide fiber membrane material are shown in Figure 2. Figure 2 (a) and Figure 2 (b) Scanning electron microscope photos of PI fibers and Ni@PI fibers in Example 1, respectively.

[0116] from Figure 2 It can be seen that the diameter of PI fiber is 1.5-2μm; after chemical nickel plating, Ni@PI fiber shows obvious changes, the diameter increases, and the metal coating is successfully coated on the PI fiber and shows good uniformity.

[0117] 3. Determination of electromagnetic shielding effectiveness of metallized polyimide fiber membrane

[0118] Figure 3 Graphs (a) and (b) show the electromagnetic shielding effectiveness and electrical conductivity of the metallized polyimide fiber membranes with and without heat pressing treatment in Examples 1 and 2.

[0119] In terms of electromagnetic shielding effectiveness, although the thickness of the Ni@PI-HP fiber membrane after hot pressing is greatly reduced, its electromagnetic shielding performance has been greatly improved. The reasons are as follows: Figure 3As shown in (b), the conductivity of Ni@PI-HP is significantly improved, which enhances the reflection of electromagnetic waves on the surface of the material, thereby improving the electromagnetic shielding performance from 29dB to 70dB. The reason for the increase in conductivity is mainly due to the closer contact between fibers after hot pressing, which greatly reduces the resistance, thereby greatly improving the conductivity of the hot-pressed PI fiber after nickel plating, thereby improving the electromagnetic shielding effectiveness.

[0120] 4. Effect of different plating time on electromagnetic shielding effectiveness and conductivity

[0121] The effects of different plating times on electromagnetic shielding effectiveness and conductivity in Example 3 are shown in the following table. Figure 4 As shown: From the data in the figure, it can be seen that as the plating time increases, the conductivity gradually increases, and the electromagnetic shielding effectiveness also increases gradually. When the plating time is extended from 25min to 30min, the conductivity of the composite fiber membrane material suddenly increases from 482S / cm to 953S / cm. This is mainly because the continuous plating layer has not yet been formed in the first 25min of plating, and between 25 and 30min, due to the self-catalytic effect of nickel, the reaction rate is accelerated, and a complete plating layer is formed on the outer surface of the fiber, so that a conductive path is formed, and the conductivity suddenly increases. However, as the plating time continues to increase, the conductivity of the composite fiber material only increases from 952S / cm at 30min to 1023S / cm at 35min, and the change is not large. This is mainly because after the complete conductive path has been formed, extending the plating time has little effect on further improving the conductivity; the electromagnetic shielding effectiveness reaches 70dB at 30min.

[0122] 5. Determination of high and low temperature resistance of metallized polyimide fiber membrane

[0123] The Ni@PI-HP prepared in Example 2 was treated at 350°C for 1 h in an air atmosphere, and then the electromagnetic shielding performance was measured. The results are as follows: Figure 5 Shown: From Figure 5 It can be seen that the electromagnetic shielding performance of Ni@PI-HP after high-temperature heat treatment is significantly improved compared with that before heat treatment. This is mainly due to the relaxation process of the metal during the heat treatment, which further compensates for the defects of the metal coating, thereby increasing the conductivity and the electromagnetic shielding effectiveness. This fully demonstrates that the metallized polyimide fiber membrane prepared by the above method has very good high temperature resistance, and the surface metal nickel layer also has extremely excellent antioxidant ability.

[0124] The Ni@PI-HP prepared in Example 2 was immersed in liquid nitrogen for 24 h, and then the electromagnetic shielding performance was measured; the results are as follows: Figure 6As shown in the figure, after liquid nitrogen treatment, the electromagnetic shielding effectiveness of Ni@PI-HP is not much different from that before treatment, which is mainly due to the strong bonding force of the coating. This also fully demonstrates that the metallized polyimide fiber membrane prepared by the method of the present invention has very good low temperature resistance.

[0125] 6. Determination of the coating bonding properties of metallized polyimide fiber membrane

[0126] The Ni@PI-HP prepared in Example 2 was bent 10,000 times and then subjected to an electromagnetic shielding effectiveness test. The results are as follows: Figure 7 As shown in the figure, it can be seen from the data that after 10,000 bends, the electromagnetic shielding performance of Ni@PI-HP is largely maintained compared with that before bending, which fully demonstrates that the metal coating of the metallized polyimide fiber film prepared by the above method has very good coating bonding strength with the polyimide matrix.

[0127] 7. Determination of corrosion resistance of metallized polyimide fiber membrane

[0128] The Ni@PI-HP after anti-corrosion treatment in Example 2 was placed in a neutral salt spray environment for 100 h and 200 h and then subjected to electromagnetic shielding effectiveness testing;

[0129] The results are as follows Figure 8 As shown in the figure, the attenuation of the electromagnetic shielding effectiveness of Ni@PI-HP after 100h and 200h of salt spray corrosion is very small compared with the previous electromagnetic shielding effectiveness, which fully demonstrates that the metallized polyimide fiber membrane prepared by the above method has very excellent corrosion resistance.

[0130] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. A method for preparing a lightweight flexible electromagnetic shielding fiber membrane material, characterized in that: The method comprises the following steps: (1) Preparation of polyamic acid salt spinning solution Dissolve the diamine and dibasic anhydride monomers in an organic solvent, stir to react with polymerization, then add an organic base, stir thoroughly, transfer to an acetone solvent to complete solvent exchange, and remove the supernatant; then take the precipitate and place it in a vacuum oven to dry to obtain polyamic acid salt, then place the polyamic acid salt in a water-alcohol mixed solution to fully dissolve it to obtain a polyamic acid salt spinning solution; (2) Preparation of polyimide fiber membrane The polyamic acid salt spinning solution obtained in step (1) is processed by an electrostatic spinning process to obtain a polyamic acid fiber membrane, and the polyamic acid fiber membrane is placed in an inert gas atmosphere for thermal imidization treatment to obtain a polyimide fiber membrane material; (3) Preparation of metallized polyimide fiber membrane The polyimide fiber membrane obtained in step (2) is first roughened in a roughening solution; then the roughened polyimide fiber membrane is immersed in an activation solution for treatment; finally, the activated polyimide fiber membrane is immersed in a plating solution for plating, washed, and dried to obtain a metallized polyimide fiber membrane material; The solute in the activation solution is chloroplatinic acid, the concentration is 0.1 ~ 20 g / L, and the activation treatment time is 30 min ~ 120 min; the plating treatment time is 10 ~ 60 min, and the temperature is 10 ~ 30 ° C; the solute in the roughening solution is one or more of dopamine, citric acid, polyphenolamine, and tannic acid; the concentration is 2 ~ 6g / L, and the treatment time is 1 h ~ 24 h; the plating solution includes a metal salt, a complexing agent, a reducing agent, and a pH regulator; (4) Corrosion resistance treatment The metallized polyimide fiber membrane material prepared in step (3) is immersed in a metal anti-corrosion treatment liquid, and then vacuum dried after the treatment.

2. The method according to claim 1, characterized in that The dianhydride monomer in step (1) is one or more of pyromellitic anhydride, biphenyl tetracarboxylic anhydride, 3,3',4,4-benzophenone tetracarboxylic anhydride, and 4,4'-oxydiphthalic anhydride; the diamine monomer is one or more of 4,4'-diaminodiphenyl ether, p-phenylenediamine, and 4,4''-diaminoterphenyl.

3. The method according to claim 1, characterized in that The organic base in step (1) is triethylamine (TEA), quinoline (QL), N,N - one or more of dimethylethanolamine (DMEA).

4. The method according to claim 1, characterized in that: The thermal imidization treatment process in step (2) also includes using a quartz plate to clamp the polyamic acid salt fiber membrane for thermal imidization treatment.

5. The method according to claim 1, characterized in that The temperature of the thermal imidization treatment in step (2) is 300-400°C and the time is 0.5-2 h.

6. The method according to claim 1, characterized in that The drying temperature in step (3) is 40 to 60°C and the drying time is 1 to 2 hours.

7. A lightweight, flexible electromagnetic shielding fiber membrane material prepared by the method described in any one of claims 1 to 6.

8. Application of the lightweight flexible electromagnetic shielding fiber membrane material according to claim 7 in the field of electromagnetic protection of aerospace devices, military equipment or precision electronic instruments.

Citation Information

Patent Citations

  • Preparation method of nickel-plated and copper-plated aromatic polyamide conductive fibers

    CN101705615A

  • Method for preparing light absorption layer of CuInSe2 (CIS) flexible thin-film solar cell

    CN102839375A