A method for preparing recyclable MXene / polyethersulfone composite microspheres and its application

In the form of composite microspheres of MXene and polyethersulfone, the MXene/polyethersulfone composite microspheres formed by electrospinning technology solve the problems of poor compatibility between MXene and polymer materials and insufficient mechanical properties, and achieve the goal of protecting against blood toxins. Effective cleaning and improved applicability.

CN116351402BActive Publication Date: 2024-10-18SICHUAN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310374636.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-18
Estimated Expiration
2043-04-10

AI Technical Summary

Technical Problem

MXene materials have poor compatibility with polymer materials soluble in organic solvents such as polyethersulfone, which limits the application of MXene in blood purification. MXene powder also has poor mechanical properties and recyclability.

Method used

It adopts the form of composite microspheres of MXene and polyethersulfone. After homogeneous preparation in N,N-dimethylacetamide solution, microspheres are formed in an electrostatic field, taking advantage of the high specific surface area and abundant surface active sites of Ti3C2. Improve adsorption performance and control microsphere diameter by adjusting electrostatic voltage and bolus speed.

Benefits of technology

It achieves the effective removal of blood toxins such as creatinine, uric acid, and bilirubin, improves the mechanical properties and recyclability of MXene, and has better compatibility with polyethersulfone, significantly improving the application effect in blood purification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116351402B_ABST
    Figure CN116351402B_ABST
Patent Text Reader

Abstract

The invention discloses a recyclable MXene / polyethersulfone composite microsphere and a preparation method thereof, belonging to the technical field of biomaterials. The microsphere is composed of an organic solution of MXene and polyethersulfone, and discloses a preparation method thereof: firstly, a MAX material is etched by lithium fluoride and hydrochloric acid, intercalated in a tetrabutylammonium hydroxide aqueous solution, and ultrasonically dissolved in an N,N-dimethylacetamide solution; then, polyethersulfone is added to the N,N-dimethylacetamide solution of the MXene for stirring, and the homogeneous solution is phase-separated in a coagulation bath by an electrostatic spinning technology to form microspheres; the microspheres can be used to prepare blood purification treatment equipment, and have good adsorption capacity for uric acid and bilirubin in the blood.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomaterials, and specifically discloses a method for preparing recyclable MXene / polyethersulfone composite microspheres and applications thereof. Background Art

[0002] MXenes are a family of two-dimensional transition metal carbonitrides, generally expressed as M n+1 X n T x , M represents an early transition metal (e.g., titanium, vanadium, niobium, molybdenum), X is carbon and / or nitrogen, n=1-3, T x Represents surface end groups such as -OH, -O- and -F. Twenty different MXenes have been synthesized so far, and more are predicted to exist. Their physical and chemical properties can be finely tuned by changing the structure and synthesis conditions. Ti3C2 is currently the most studied MXene because of its mild etching conditions and good biocompatibility. Polyethersulfone has good mechanical properties and acid and alkali resistance, and is a commercial polymer raw material widely used in the field of blood purification technology.

[0003] Polyethersulfone materials are often used as the substrate of blood purification materials because of their good mechanical properties and blood compatibility, but because of their poor adsorption performance for toxins in the blood, the polyethersulfone substrate needs to be modified. MXene, as a two-dimensional layered material, has a large specific surface area, and during the etching process of HCl and LiF, the surface of MXene is easy to obtain rich oxygen-containing surface groups, which is conducive to the adsorption of toxin molecules in the blood, such as creatinine, uric acid, urea, bilirubin, etc.

[0004] MXene materials, when applied in powder form, have poor mechanical properties and are difficult to recycle, which greatly limits their application in blood purification. Therefore, it is a simple solution to combine them with polymer materials and apply them in the form of microspheres. During electrospinning, polyethersulfone usually needs to be dissolved in an organic solvent, but the solubility of MXene materials in organic solvents is poor and the compatibility of MXene with polymer materials is poor. This limits the comprehensive application of MXene. Summary of the invention

[0005] One of the purposes of the present invention is to solve the problem of poor compatibility between MXene materials and polymer materials soluble in organic solvents such as polyethersulfone, and to provide a feasible improvement method for further application of MXene materials. The present invention is achieved by the following technical means:

[0006] The present invention discloses a recyclable MXene / polyethersulfone composite microsphere, comprising:

[0007] The mass ratio of MXene to polyethersulfone is 1:(50-200);

[0008] After the N,N-dimethylacetamide solution of MXene is mixed with polyethersulfone to form a homogeneous solution, the mass ratio of the sum of the masses of MXene and polyethersulfone in the solution to the mass of the solvent N,N-dimethylacetamide solution is (14-16):(84-86).

[0009] Furthermore, the MAX phase material is Ti3AlC2; and the MXene material is Ti3C2.

[0010] Furthermore, the N,N-dimethylacetamide solution of Ti3C2 is prepared by the following method:

[0011] 1) Quantitatively weigh 1-1.6 g LiF, dissolve it in 20 mL 9 mol / L hydrochloric acid, and stir in a polytetrafluoroethylene beaker until it is completely dissolved; weigh 1 g Ti3AlC2 powder, add it to the solution in small amounts several times, and stir at 35°C for 24-48 hours to obtain a first solution;

[0012] 2) transferring the first solution to a centrifuge tube, centrifuging at 4000 rpm, taking a precipitate, and then washing it twice with 1 mol / L dilute hydrochloric acid, washing the precipitate with deionized water until the pH of the supernatant after centrifugation is greater than or equal to 6, and the precipitate swells significantly, and freeze-drying it for 24 hours to obtain a freeze-dried precipitate;

[0013] 3) Take 1 g of freeze-dried precipitate in a beaker, add 15 mL of 25% wt tetrabutylammonium hydroxide solution, and stir at 30°C for more than 8 hours to perform intercalation reaction;

[0014] 4) After the intercalation is completed, the above system is placed in a centrifuge tube for centrifugation, the precipitate is washed twice with ethanol, and then N, N-dimethylacetamide solution is added, shaken well, ultrasonicated for 30 minutes, and centrifuged to obtain N, N-dimethylacetamide solution of Ti3C2;

[0015] 5) The content of Ti3C2 in the solution is determined by filtering 1 mL of the above-mentioned N,N-dimethylacetamide solution of Ti3C2, vacuum drying, and then weighing to determine the concentration, unit: mg / mL.

[0016] The present invention also discloses a method for preparing any of the above MXene / polyethersulfone composite microspheres, comprising:

[0017] 1) Preparation of MXene / polyethersulfone composite microsphere forming liquid:

[0018] Add polyethersulfone to N,N-dimethylacetamide solution, stir for 2-8h at room temperature to obtain polyethersulfone solution, add Ti3C2 N,N-dimethylacetamide solution to the polyethersulfone solution, stir for 20-30min to obtain spherical liquid;

[0019] 2) Preparation of MXene / polyethersulfone composite microspheres:

[0020] The prepared spheroidizing liquid is drawn into a syringe, and the syringe is pushed in an electrostatic field, so that the spheroidizing liquid forms droplets that fall into a coagulation bath to undergo a phase transition, thereby obtaining MXene / polyethersulfone composite microspheres.

[0021] Furthermore, in step 2), the electrostatic field is formed by an electrospinning machine, and the diameter of the microspheres is controlled by adjusting the electrostatic voltage, the syringe needle or the injection speed.

[0022] Furthermore, the coagulation bath in step 2) is a mixed solvent of deionized water and ethanol.

[0023] The present invention also discloses a MXene / polyethersulfone composite microsphere prepared according to any of the above preparation methods.

[0024] The present invention also discloses an application of any of the above-mentioned MXene / polyethersulfone composite microspheres in the preparation of a blood purification device.

[0025] Furthermore, the blood purification device includes: blood purification for those with bilirubin, creatinine and uric acid clearance disorders.

[0026] The ultimate goal of the present invention is to apply the MXene / polyethersulfone composite microspheres to the adsorption of toxins in the blood. Therefore, the blood purification of patients with abnormal renal metabolism should be tested for the adsorption capacity of toxins in the blood. MXene is evenly distributed in the porous matrix of polyethersulfone, providing good adsorption performance for the microspheres. At the same time, MXene and polyethersulfone both have good blood compatibility. The adsorption performance is based on the adsorption characteristics brought by the large specific surface area and abundant surface active sites of MXene.

[0027] Compared with the prior art, the advantages of the present invention are:

[0028] 1. The inventors used Ti3C2 / polyethersulfone composite microspheres to conduct clearance tests on three blood toxins: creatinine, uric acid, and bilirubin, and found that the microspheres can effectively clear all of the above blood toxins.

[0029] 2. The present invention provides a method for practical application of Ti3C2-type MXene in the field of blood purification. After MXene is compounded with polyethersulfone, it has better mechanical properties than MXene powder and is easier to apply and recycle.

[0030] 3. Compared with the traditional method of dispersing Ti3C2 in an organic solvent by ultrasound, the Ti3C2 formed by this method has better compatibility with polyethersulfone, and Ti3C2 is more evenly dispersed in polyethersulfone. After testing, the MXene / polyethersulfone composite microspheres have good scavenging ability for creatinine, uric acid and bilirubin. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a scanning electron microscope image of the intercalated MXene of an embodiment of the present invention;

[0032] Figure 2 This is a cross-sectional scanning electron microscope image of the MXene / polyethersulfone composite microspheres prepared in an embodiment of the present invention;

[0033] Figure 3 The creatinine clearance capacity of the microspheres in the embodiment;

[0034] Figure 4 The scavenging ability of the microspheres on uric acid in the example;

[0035] Figure 5 The bilirubin clearance ability of the microspheres in the examples. DETAILED DESCRIPTION

[0036] The present invention will be further described below in conjunction with the accompanying drawings.

[0037] The adsorption performance test method of the microspheres prepared in Examples 1-3 of the present invention is:

[0038] (1) Creatinine adsorption performance test:

[0039] A concentration-absorbance standard curve was established using 10 mg / L, 5 mg / L, 2.5 mg / L, and 1.25 mg / mL creatinine solutions. 20 mg of the microspheres were placed in 20 ml of creatinine solution (50 mg / L) on a shaker and kept at 37°C in the dark for 6 h. The absorbance of the adsorbed solution at 232 nm was measured using an ultraviolet spectrophotometer. The adsorption amount of the microspheres was calculated according to the Lambert-Beer law. The results are as follows: Figure 3 As shown;

[0040] (2) Uric acid adsorption performance test:

[0041] A concentration-absorbance standard curve was established using 50 μmol / L, 25 μmol / L, 12.5 μmol / L, and 6.25 μmol / L uric acid solutions; 20 mg of microspheres were placed in 20 mL of uric acid solution (250 μmol / L) on a shaker, and kept at 37°C in the dark for 6 h. The absorbance of the adsorbed solution at 293 nm was measured using an ultraviolet spectrophotometer, and the adsorption amount of the microspheres was calculated according to the Lambert-Beer law. The results are as follows: Figure 4 As shown;

[0042] (3) Bilirubin adsorption performance test:

[0043] A concentration-absorbance standard curve was established using 15 mg / L, 7.5 mg / L, 3.75 mg / L, and 1.875 mg / L bilirubin solutions; 20 mg of the wet weight of microspheres was placed in 20 mL of bilirubin solution (150 mg / L), kept at 37°C in a dark environment for 6 hours, and then the absorbance of the adsorbed solution at 438 nm was measured using an ultraviolet spectrophotometer. The adsorption amount of the microspheres was calculated according to the Lambert-Beer law. The results are as follows: Figure 5 shown.

[0044] The N,N-dimethylacetamide solution of MXene in the following Examples 1-3 is prepared by:

[0045] 1) Quantitatively weigh 1.6g LiF, dissolve it in 20ml 9mol / L hydrochloric acid, and stir in a polytetrafluoroethylene beaker until it is completely dissolved; weigh 1g Ti3AlC2 powder, add it to the solution in small amounts several times, and stir at 35°C for 36h;

[0046] 2) The reaction solution was transferred to a centrifuge tube, centrifuged at 4000 rpm, and the precipitate was taken. Then, the precipitate was washed twice with 1 mol / L dilute hydrochloric acid, shaken, centrifuged, and the precipitate was taken. The precipitate was then washed with deionized water until the pH of the supernatant was ≥ 6, and after the precipitate was obviously swollen, the material was freeze-dried for 24 hours;

[0047] 3) Take 1 g of the freeze-dried precipitate in a beaker, add 15 mL of 25% wt tetrabutylammonium hydroxide solution, and stir at 30°C for 8 h to perform intercalation reaction;

[0048] 4) After the intercalation is completed, the above system is placed in a centrifuge tube for centrifugation, the precipitate is washed twice with ethanol, and then 10 mL of N, N-dimethylacetamide solution is added, shaken well, ultrasonicated for 30 minutes, and centrifuged to obtain N, N-dimethylacetamide solution of Ti3C2;

[0049] The above-mentioned intercalated MXene has a larger flake structure, such as Figure 1 shown.

[0050] Example 1

[0051] In this embodiment, the mass ratio of MXene to polyethersulfone is 1:150. 1950 mg of polyethersulfone is dissolved in 11087 mg of N,N-dimethylacetamide solution and stirred at room temperature for 4 hours to form a homogeneous polyethersulfone solution. Then, 1 mL of MXene N,N-dimethylacetamide solution is added thereto and stirred at room temperature for 30 minutes to mix to obtain a spherical liquid. The spherical liquid is loaded into a syringe and electrosprayed under an electrostatic field to smoothly form droplets. Phase separation occurs rapidly in a coagulation bath of water and ethanol (volume ratio 1:3) to form microspheres of uniform size. The microspheres are soaked in PBS buffer for use. The scanning electron microscope image of the interior of the microspheres after drying is as follows: Figure 2 As shown, from Figure 2 It can be seen that the microspheres have a porous structure inside and there are MXene flake wrinkles on the pore walls.

[0052] The creatinine clearance, uric acid clearance and bilirubin clearance capacity tests were performed according to the above method, and the results are shown in Figure 3-5 As can be seen from the figure, the microspheres of this embodiment have the ability to clear creatinine, uric acid and bilirubin.

[0053] Example 2

[0054] This example aims to illustrate the effect of MXene content on the effect of MXene / polyethersulfone composite microspheres in removing blood endotoxins. In this example, the mass ratio of MXene to polyethersulfone is 1:100.

[0055] 1300 mg of polyethersulfone was dissolved in 7094 mg of N,N-dimethylacetamide solution, stirred at room temperature for 4 hours to form a homogeneous polyethersulfone solution, and then 1 mL of MXene N,N-dimethylacetamide solution was added thereto, stirred at room temperature for 30 minutes to mix, and a spherical liquid was obtained; the spherical liquid was loaded into a syringe, and electrosprayed under an electrostatic field to smoothly form droplets, and phase separation occurred rapidly in a coagulation bath of water and ethanol (volume ratio 1:3) to form microspheres of uniform size. The microspheres were soaked in PBS buffer for use. The microspheres have a porous structure inside, and there are flaky wrinkles of MXene on the pore walls.

[0056] The creatinine clearance, uric acid clearance and bilirubin clearance capacity tests were performed according to the above method, and the results are shown in Figure 3-5 As can be seen from the figure, the microspheres of this embodiment have the ability to clear creatinine, uric acid and bilirubin, and the clearing performance is improved compared with Example 1.

[0057] Example 3

[0058] This example aims to illustrate the effect of MXene content on the effect of MXene / polyethersulfone composite microspheres in removing blood endotoxins. In this example, the mass ratio of MXene to polyethersulfone is 1:75.

[0059] 974 mg of polyethersulfone was dissolved in 5092 mg of N,N-dimethylacetamide solution, stirred at room temperature for 4 hours to form a homogeneous polyethersulfone solution, and then 1 ml of MXene N,N-dimethylacetamide solution was added thereto, stirred at room temperature for 30 minutes to mix, and a spherical liquid was obtained; the spherical liquid was loaded into a syringe, and electrosprayed under an electrostatic field to smoothly form droplets, and phase separation occurred rapidly in a coagulation bath of water and ethanol (volume ratio 1:3) to form microspheres of uniform size. The microspheres were soaked in PBS buffer for use. The microspheres have a porous structure inside, and there are flaky wrinkles of MXene on the pore walls.

[0060] The creatinine clearance, uric acid clearance and bilirubin clearance capacity tests were performed according to the above method, and the results are shown in Figure 3-5 As can be seen from the figure, the microspheres of this embodiment have the ability to clear creatinine, uric acid and bilirubin, and the clearing performance is improved compared with Examples 1 and 2.

Claims

1. Application of recyclable MXene / polyethersulfone composite microspheres in the preparation of blood purification equipment, wherein: In the recyclable MXene / polyethersulfone composite microspheres, the mass ratio of MXene to polyethersulfone is 1:(50-200); After the N,N-dimethylacetamide solution of MXene is mixed with polyethersulfone to form a homogeneous solution, the mass ratio of the sum of the mass of MXene and polyethersulfone in the solution to the mass of the solvent N,N-dimethylacetamide solution is (14-16): (84-86); The N,N-dimethylacetamide solution of the MXene was prepared by the following method: 1) Etching the MAX raw material in a solution of HCl and LiF, washing it with deionized water for multiple times to obtain a multi-layer MXene material, and freeze-drying it for later use; 2) adding the multilayer MXene material to a tetrabutylammonium hydroxide solution and stirring for more than 8 hours, centrifuging after intercalation, and washing twice with anhydrous ethanol to obtain a washed multilayer MXene material; 3) Add 20 mL of N,N-dimethylacetamide solution to the cleaned multilayer MXene material and dissolve it by ultrasonication to obtain MXene solution in N,N-dimethylacetamide.

2. The use according to claim 1, wherein: The MAX phase material is Ti3AlC2; The MXene material is Ti3C2.

3. The use according to claim 1, wherein: Step 3) The MXene content in the N,N-dimethylacetamide solution of MXene is determined by the following method: Take 1 mL of MXene N,N-dimethylacetamide solution, filter it, and after vacuum drying, determine the concentration of MXene in the MXene N,N-dimethylacetamide solution, unit: mg / mL.

4. A method for preparing recyclable MXene / polyethersulfone composite microspheres, comprising: 1) Preparation of MXene / polyethersulfone composite microsphere forming liquid: Add polyethersulfone to N,N-dimethylacetamide solution, stir at room temperature for 2-8 hours to obtain polyethersulfone solution, add MXene N,N-dimethylacetamide solution to the polyethersulfone solution, stir for 20-30 minutes to obtain spherical liquid; 2) Preparation of MXene / polyethersulfone composite microspheres: The prepared spheroidizing liquid is drawn into a syringe, and the syringe is pushed in an electrostatic field, so that the spheroidizing liquid forms droplets and falls into a coagulation bath to undergo phase conversion, thereby obtaining MXene / polyethersulfone composite microspheres; wherein: The N,N-dimethylacetamide solution of the MXene was prepared by the following method: ① Etch the MAX raw material in a solution of HCl and LiF, wash it with deionized water for multiple times to obtain a multi-layer MXene material, and freeze-dry it for later use; ② Add the multilayer MXene material to a tetrabutylammonium hydroxide solution and stir for more than 8 hours. After intercalation, centrifuge and wash twice with anhydrous ethanol to obtain a washed multilayer MXene material; ③ Add 20 mL of N,N-dimethylacetamide solution to the cleaned multilayer MXene material and dissolve it by ultrasonication to obtain MXene solution in N,N-dimethylacetamide.

5. The preparation method according to claim 4, wherein: Step 2) The electrostatic field is formed by an electrospinning machine, and the diameter of the microspheres is controlled by adjusting the electrostatic voltage, the syringe needle or the injection speed.

6. The preparation method according to claim 4, wherein: The coagulation bath in step 2) is a mixed solvent of deionized water and ethanol.

7. A recyclable MXene / polyethersulfone composite microsphere prepared according to any one of the preparation methods of claims 4-6.

Citation Information

Patent Citations

  • Porous polymer nanoparticle and preparation method thereof

    CN101735613A

  • Absorbing material and method for manufacturing same, absorbing sheet, separation membrane for artificial dialysis, and artificial dialyzer

    WO2022163583A1