Carbon fiber nano-surface modification device and method
Through the combination of carbon fiber conveying roller group and ultrasonic dispersion tank, carbon fiber power-on self-heating heating technology is used to solve the problems of high energy consumption of the outer wall heating device of the high-temperature reactor and slow carbon fiber heating, achieving efficient carbon fiber nanosurface modification, reducing energy Consumption and cost.
Patent Information
- Application Number
- CN202310441499.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-23
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-04-23
AI Technical Summary
The existing high-temperature reactor outer wall heating device has high energy consumption, large furnace volume, and slow carbon fiber heating.
Carbon fiber conveying roller set, ultrasonic dispersion tank and reactor are used to heat the carbon fiber by energizing and self-heating, combined with the carbon nanotube growth heating circuit, to achieve rapid heating of carbon fiber and reach the reaction temperature within a small range, reducing heat loss and the use of thermal insulation materials.
It reduces the cost and energy consumption of high-temperature furnaces, shortens the carbon fiber heating time, reduces the reactor volume and the use of insulation materials, and improves the heat utilization rate.
Smart Images

Figure CN116356558B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of carbon fiber production, and in particular relates to a carbon fiber nano-surface modification device and method. Background Art
[0002] Carbon fiber is an inorganic non-metallic reinforcing fiber with high strength, high modulus and low density. It is mainly used as a reinforcing agent in the manufacture of composite materials. An important aspect of composite material manufacturing is the interface bonding between the reinforcing agent and the matrix. If the interface bonding is good, the role of the reinforcing agent can be fully exerted and the composite material has excellent performance. Carbon fiber surface treatment generally adopts chemical methods, that is, functional groups are generated on the surface of carbon fiber through chemical reactions. These functional groups make the carbon fiber and the matrix tightly bonded. Another way to improve the interfacial bonding strength is to increase the roughness of the carbon fiber surface so that a geometric slip barrier is formed at the interface between the matrix and the carbon fiber. This method generates defects or grows nanofibers or particles on the surface of carbon fiber. The methods used include coating method, corrosion method, etching method and high temperature deposition method. Among them, the high temperature deposition method can generate nanostructured materials such as carbon nanotubes on the surface of carbon fiber, so that the interface of the composite material forms a pin structure, and the bonding strength is greatly improved. It is a new surface treatment method.
[0003] In the high-temperature deposition method, the current process is to introduce the carbon fiber tow into a high-temperature furnace and complete the surface modification after a certain period of reaction. The disadvantage of this method is that the energy consumption is relatively high, because the high-temperature furnace is heated by the outer wall of the furnace, the loss caused by heat loss is very large, and the heat utilization rate is not high. This high-temperature furnace heated by the outer wall requires a heating element and more insulation materials, and the furnace is bulky. In addition, it takes a certain amount of time for the heat to be transferred from the furnace wall to the carbon fiber, which is inefficient. Summary of the invention
[0004] In view of this, one of the purposes of the present invention is to propose a carbon fiber nano-surface modification device to address the shortcomings of the current high-temperature reactor outer wall heating device, which has high energy consumption, large furnace volume, and slow carbon fiber heating.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A carbon fiber nano-surface modification device comprises a carbon fiber conveying roller set, a carbon fiber etching heating circuit, a carbon nanotube growth heating circuit, an ultrasonic dispersion tank and a reaction furnace;
[0007] The carbon fiber passes through the ultrasonic dispersion tank and the reaction furnace in sequence through the carbon fiber conveying roller group;
[0008] The carbon fiber conveying roller group includes fiber powered transmission rollers located at the front and rear ends of the reaction furnace. The fiber powered transmission rollers are respectively connected to the carbon fiber etching heating circuit or the carbon nanotube growth heating circuit, and form a loop heating with the carbon fibers therebetween.
[0009] Furthermore, the carbon fiber conveying roller group also includes a carbon fiber unwinding roller, a fiber transmission roller, a clustering ring and a carbon fiber collecting roller;
[0010] The carbon fiber is released through the carbon fiber unwinding roller, then enters and exits the ultrasonic dispersion tank through the fiber driving roller, then enters and exits the reaction furnace through the fiber electrified driving roller, and finally enters the carbon fiber collecting roller for collection through the bunching ring.
[0011] Furthermore, a partition is provided inside the reaction furnace, and the partition divides the reaction furnace into an etching area and a carbon nanotube growth area according to the moving direction of the carbon fiber.
[0012] Furthermore, the reaction furnace is provided with an etching gas inlet in the etching area; and the reaction furnace is provided with a carbon nanotube reaction gas inlet in the carbon nanotube growth area.
[0013] Another object of the present invention is to provide a method for surface modification of carbon fiber nanostructures using the above device, comprising the following steps:
[0014] (1) Spreading of carbon fiber tows: The carbon fiber is released through the carbon fiber release roller, and then enters and exits the ultrasonic dispersion tank through the fiber transmission roller. The ultrasonic wave in the ultrasonic dispersion tank spreads the carbon fiber to a certain width;
[0015] (2) The fiber powered transmission roller guides the carbon fiber into the reaction furnace and heats it by power;
[0016] (3) introducing an etchant into the etching zone of the reaction furnace to etch defective structures on the surface;
[0017] (4) introducing ferrocene into the carbon nanotube growth zone of the reactor to grow carbon nanotubes on the surface of the etched carbon fiber;
[0018] (5) The modified carbon fiber enters the carbon fiber collecting roller through the bunching ring to collect the surface-modified carbon fiber product.
[0019] Furthermore, the carbon fiber is a carbon fiber tow having no sizing agent on the surface.
[0020] Furthermore, the medium for ultrasonic expansion in step (1) is water, the expansion time is 2-5 minutes, the ultrasonic frequency is 0.1-0.3 MHz, and the applied power is 0.3-0.6 W.
[0021] Furthermore, the width of the expanded carbon fiber tow in step (1) is 0.5-0.8 m.
[0022] Furthermore, the etchant in step (3) is a mixture of hydrogen and nitrogen; the volume ratio of hydrogen to nitrogen is between 1:0.1 and 1:0.7, the reaction temperature is between 500 and 800° C., and the etching time is 4 to 10 minutes.
[0023] Furthermore, in step (4), the mass ratio of ferrocene to carbon fiber is between 0.02:1 and 0.05:1, the carbon nanotube generation temperature is between 700 and 1000° C., and the generation time is 6 to 15 minutes.
[0024] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0025] The resistivity of carbon fiber is within the resistance range of resistance heating elements. Therefore, the method of self-heating by powering on can be used to quickly heat up the carbon fiber itself. The advantages of this method are that the self-heating heating method does not require the heating element components of a traditional high-temperature furnace, reducing the cost of the high-temperature furnace; self-heating eliminates the heat transfer process from the furnace to the carbon fiber, so the temperature rises quickly; since the reaction temperature is only reached in a small range around the carbon fiber, the furnace wall temperature of the reactor is low, heat loss is small, energy consumption is low, and less insulation material is required.
[0026] The resistivity of carbon materials is between that of metal conductors and insulators, so they are often used as high-temperature heating materials. Carbon fiber is a fibrous material composed of carbon elements with a resistance range of 10 -2 -10 2 The present invention utilizes the characteristic that electric current can directly flow through carbon fiber to generate heat to a very high temperature (the melting point of carbon is higher than 3000℃). In the process of etching the carbon fiber surface and growing carbon nanotubes, the method of directly heating the carbon fiber by electric current can be used. The heat transfer process from the heating element of the high-temperature furnace to the carbon fiber can be eliminated. The carbon fiber will heat up very quickly, reducing the heating time of the carbon fiber, thereby shortening the length of the furnace. Moreover, since the heating element material of the conventional high-temperature furnace is not required, the cost is greatly reduced. Since the temperature in the center of the furnace is the highest and the temperature of the furnace wall is relatively low, the heat loss is very small, and the use of insulation materials is also reduced, and the volume of the reaction furnace is greatly reduced.
[0027] Carbon fiber is used as a tow composed of thousands of single fibers. In order to make the surface of the carbon fiber react evenly, the carbon fiber needs to be spread out so that there are certain gaps between the carbon fibers to allow the reaction gas to diffuse to the surface of the carbon fiber. The present invention uses an ultrasonic dispersion method to spread out the carbon fiber tow, and can achieve full and uniform dispersion of the carbon fiber in water. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0029] Figure 1 This is a schematic front view of a carbon fiber nano-surface modification device provided by the present invention.
[0030] Figure 2 This is a schematic top view of a carbon fiber nano-surface modification device provided by the present invention.
[0031] Figure 1 middle:
[0032] 1. Carbon fiber unwinding roller, 2. Fiber driving roller, 3. Ultrasonic dispersion tank, 4. Fiber energizing driving roller, 5. Etching gas inlet, 6. Etching zone, 7. Partition, 8. Carbon nanotube reaction gas inlet, 9. Carbon nanotube growth zone, 10. Bunching ring, 11. Carbon fiber collecting roller, 12. Carbon fiber etching heating circuit, 13. Carbon nanotube growth heating circuit. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] like Figure 1-2 As shown, the present invention discloses a carbon fiber nano-surface modification device, including a carbon fiber conveying roller group, an ultrasonic dispersion tank 3 and a reaction furnace; the carbon fiber conveying roller group includes a fiber electrified transmission roller 4, and the fiber electrified transmission roller 4 includes four transmission rollers, which are respectively arranged at the front and rear inlet and outlet ends outside the reaction furnace and inside the furnace, and the electrified transmission rollers and the carbon fibers in the furnace form two current loops, namely, a carbon fiber etching heating loop 12 and a carbon nanotube growth heating loop 13, and form a loop heating with the carbon fibers therebetween.
[0035] Further, in order to improve the above technical solution, the carbon fiber conveying roller group includes a carbon fiber unwinding roller 1, a fiber transmission roller 2, a clustering ring 10 and a carbon fiber receiving roller 11;
[0036] The carbon fiber is released through the carbon fiber unwinding roller 1, and the fiber driving roller 2 includes four driving rollers, two of which are respectively arranged at the front and rear ends of the ultrasonic dispersion tank 3, and the other two are arranged inside the ultrasonic dispersion tank 3. The carbon fiber enters and exits the ultrasonic dispersion tank 3 under the drive of the fiber driving roller 2, and the dispersed carbon fiber enters and exits the reaction furnace under the drive of the fiber energized driving roller 4, and finally enters the carbon fiber collecting roller 11 through the bunching ring 10 for collecting.
[0037] Furthermore, in order to improve the above technical solution, a partition 7 is provided inside the reaction furnace, and the partition 7 divides the reaction furnace into an etching area 6 and a carbon nanotube growth area 9 according to the moving direction of the carbon fiber.
[0038] Furthermore, in order to improve the above technical solution, the reaction furnace is provided with an etching gas inlet 5 in the etching area 6 ; and the reaction furnace is provided with a carbon nanotube reaction gas inlet 8 in the carbon nanotube growth area 9 .
[0039] Compared with the conventional outer wall heating reaction furnace device, the length of the device of the present invention is reduced by 22%; the thickness of the heat insulation material of the high temperature furnace is reduced from 50mm to 20mm.
[0040] The present invention takes polyacrylonitrile-based carbon fiber T300 as an example for surface modification. However, the invention does not limit the type and brand of carbon fiber. The strength of carbon fiber is tested in accordance with GB / T3362-2017 "Test Method for Tensile Properties of Carbon Fiber Multifilaments". Since the test of carbon fiber strength is to make the carbon fiber into a composite material rod, the strength is increased after surface modification, that is, the strength of the carbon fiber is brought into play.
[0041] Example 1
[0042] A method for performing carbon fiber nano-surface modification using the above device comprises the following steps:
[0043] (1) Spreading of carbon fiber tows: 12K T300 polyacrylonitrile carbon fiber was released through a carbon fiber release roller, and then passed through a fiber transmission roller to enter and exit an ultrasonic dispersion tank. The ultrasonic frequency was 0.3 MHz, the applied power was 0.4 W, the expansion time was 2 minutes, and the width of the carbon fiber tow after expansion was 0.5 m.
[0044] (2) The fiber powered transmission roller guides the carbon fiber into the reaction furnace and heats it by power;
[0045] (3) Introducing an etchant, i.e., a mixture of hydrogen and nitrogen, into the etching zone of the reactor; the volume ratio of the etchant hydrogen and nitrogen is 1:0.1, the volume: mass ratio of the etching gas to the introduced carbon fiber is 0.4 liters: 1 gram of carbon fiber, the etching temperature is 650° C., the etching is performed for 4 minutes, and the defect structure is etched on the surface;
[0046] (4) introducing ferrocene into the carbon nanotube growth zone of the reactor, wherein the mass ratio of the introduced ferrocene to the carbon fiber is 0.02:1, the carbon nanotube generation temperature is 850° C., the generation time is 6 minutes, and the carbon nanotubes are grown on the surface of the etched carbon fiber;
[0047] (5) The modified carbon fiber enters the carbon fiber collecting roller through the bunching ring to collect the surface-modified carbon fiber product.
[0048] After modification, the carbon fiber gained 0.5% in weight and had a strength of 3.75 GPa, which was 8.1% higher than the unmodified carbon fiber's 3.47 GPa. When the surface modification of 1000 meters of carbon fiber was completed, compared with the traditional outer wall heating reactor, the power consumption of the surface modification in this embodiment was reduced from 5.1 kW.h to 2.3 kW.h.
[0049] Example 2
[0050] A method for performing carbon fiber nano-surface modification using the above device comprises the following steps:
[0051] (1) Spreading of carbon fiber tows: 12K T300 polyacrylonitrile carbon fiber was released through a carbon fiber pay-off roller, and then passed through a fiber transmission roller to enter and exit an ultrasonic dispersion tank. The ultrasonic frequency was 0.2 MHz, the applied power was 0.6 W, and the expansion time was 3.5 minutes. The width of the expanded carbon fiber tow was 0.6 m.
[0052] (2) The fiber powered transmission roller guides the carbon fiber into the reaction furnace and heats it by power;
[0053] (3) Introducing an etchant, i.e., a mixture of hydrogen and nitrogen, into the etching zone of the reactor; the volume ratio of the etchant hydrogen and nitrogen is 1:0.7, the volume:mass ratio of the etching gas to the introduced carbon fiber is 0.5 liters: 1 gram of carbon fiber, the etching temperature is 500° C., the etching is performed for 7 minutes, and the defect structure is etched on the surface;
[0054] (4) introducing ferrocene into the carbon nanotube growth zone of the reactor, wherein the mass ratio of the introduced ferrocene to the carbon fiber is 0.035:1, the carbon nanotube generation temperature is 1000° C., the generation time is 10.5 minutes, and the carbon nanotubes are grown on the surface of the etched carbon fiber;
[0055] (5) The modified carbon fiber enters the carbon fiber collecting roller through the bunching ring to collect the surface-modified carbon fiber product.
[0056] After modification, the carbon fiber gained 1.3% in weight and had a strength of 3.93 GPa, which was 13.3% higher than the unmodified carbon fiber's 3.47 GPa. When the surface modification of 1000 meters of carbon fiber was completed, compared with the traditional outer wall heating reactor, the power consumption of the surface modification in this embodiment was reduced from 7.4 kW.h to 3.3 kW.h.
[0057] Example 3
[0058] A method for performing carbon fiber nano-surface modification using the above device comprises the following steps:
[0059] (1) Spreading of carbon fiber tows: 12K T300 polyacrylonitrile carbon fiber was released through a carbon fiber pay-off roller, and then passed through a fiber transmission roller to enter and exit an ultrasonic dispersion tank. The ultrasonic frequency was 0.1 MHz, the applied power was 0.3 W, and the expansion time was 5 minutes. The width of the expanded carbon fiber tow was 0.8 m.
[0060] (2) The fiber powered transmission roller guides the carbon fiber into the reaction furnace and heats it by power;
[0061] (3) Introducing an etchant, i.e., a mixture of hydrogen and nitrogen, into the etching zone of the reactor; the volume ratio of the etchant hydrogen and nitrogen is 1:0.5, the volume:mass ratio of the etching gas to the introduced carbon fiber is 0.2 liters: 1 gram of carbon fiber, the etching temperature is 800°C, the etching is performed for 10 minutes, and the defect structure is etched on the surface;
[0062] (4) introducing ferrocene into the carbon nanotube growth zone of the reactor, wherein the mass ratio of the introduced ferrocene to the carbon fiber is 0.05:1, the carbon nanotube generation temperature is 700° C., the generation time is 15 minutes, and the carbon nanotubes are grown on the surface of the etched carbon fiber;
[0063] (5) The modified carbon fiber enters the carbon fiber collecting roller through the bunching ring to collect the surface-modified carbon fiber product.
[0064] After modification, the carbon fiber gained 1.8% in weight and had a strength of 4.12 GPa, which was 18.7% higher than the unmodified carbon fiber's 3.47 GPa. When the surface modification of 1000 meters of carbon fiber was completed, compared with the traditional outer wall heating reactor, the power consumption of the surface modification in this embodiment was reduced from 11.3 kW.h to 5.2 kW.h.
[0065] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0066] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for surface modification of carbon fiber nanoparticles, characterized in that: The carbon fiber nano-surface modification device includes a carbon fiber conveying roller group, a carbon fiber etching heating circuit, a carbon nanotube growth heating circuit, an ultrasonic dispersion tank and a reaction furnace; The carbon fiber passes through the ultrasonic dispersion tank and the reaction furnace in sequence through the carbon fiber conveying roller group; The carbon fiber conveying roller group includes a fiber electrified transmission roller, which is located at the front and rear ends of the reaction furnace. The fiber electrified transmission roller is respectively connected to the carbon fiber etching heating circuit or the carbon nanotube growth heating circuit, and the carbon fiber therebetween forms a loop for heating; The carbon fiber nano-surface modification method comprises the following steps: (1) Spreading of carbon fiber tows: Ultrasonic technology is used to expand the carbon fiber; the expansion medium is water, the ultrasonic frequency is 0.1-0.3MHz, the applied power is 0.3-0.6W, the expansion time is 2-5 minutes, and the width of the expanded carbon fiber tow is 0.5-0.8m; (2) introducing carbon fiber into a reaction furnace and heating it by electricity; (3) introducing an etchant into the etching zone of the reaction furnace to etch defective structures on the surface; (4) introducing ferrocene into the carbon nanotube growth zone of the reactor to grow carbon nanotubes on the surface of the etched carbon fiber; (5) Collecting surface-modified carbon fiber products.
2. A carbon fiber nano-surface modification method according to claim 1, characterized in that: The carbon fiber conveying roller group also includes a carbon fiber unwinding roller, a fiber transmission roller, a clustering ring and a carbon fiber collecting roller; The carbon fiber is released through the carbon fiber unwinding roller, then enters and exits the ultrasonic dispersion tank through the fiber driving roller, enters and exits the reaction furnace through the fiber electrified driving roller, and finally enters the carbon fiber collecting roller for collection through the bunching ring.
3. A carbon fiber nano-surface modification method according to claim 1 or 2, characterized in that: A partition is arranged inside the reaction furnace, and the partition divides the reaction furnace into an etching area and a carbon nanotube growth area according to the moving direction of the carbon fiber.
4. A carbon fiber nano-surface modification method according to claim 3, characterized in that: The reaction furnace is provided with an etching gas inlet in the etching area; and the reaction furnace is provided with a carbon nanotube reaction gas inlet in the carbon nanotube growth area.
5. A carbon fiber nano-surface modification method according to claim 1, characterized in that: The carbon fiber is a carbon fiber tow with no sizing agent on the surface.
6. A carbon fiber nano-surface modification method according to claim 1, characterized in that: The etchant in step (3) is a mixture of hydrogen and nitrogen; the volume ratio of hydrogen:nitrogen is between 1:0.1 and 1:0.7, the volume:mass ratio of etching gas to introduced carbon fiber is between 0.2-0.5L:1g, the reaction temperature is between 500 and 800°C, and the etching time is 4 to 10 minutes.
7. A carbon fiber nano-surface modification method according to claim 1, characterized in that: In step (4), the mass ratio of ferrocene to carbon fiber is between 0.02:1 and 0.05:1, the carbon nanotube generation temperature is between 700 and 1000° C., and the generation time is 6 to 15 minutes.