Water-soluble film, manufacturing method and packaging body

By adjusting the contact angle, swelling and complete dissolution time of the water-soluble film, combined with heat sealing treatment, the problem of the reduction of sealing strength of the water-soluble film during long-term storage and transportation is solved, ensuring the stability and safety of the drug packaging body.

CN116368076BActive Publication Date: 2024-11-12KURARAY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280007176.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-10-01
Filing Date
2022-09-30
Publication Date
2024-11-12
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

The existing water-soluble films are prone to the problem of reduced seal strength during long-term storage and transportation, especially in the case of sea transportation and long-term storage, which leads to a decrease in the seal strength of the heat sealing part of the packaging body, affecting the packaging effect of the agent.

Method used

By adjusting the composition of the water-soluble film and film-making conditions, ensuring contact angle, swelling and complete dissolution time within a specific range, combined with appropriate heat sealing treatment, a water-soluble film with excellent sealing strength is prepared. Specific measures include deionized water droplet addition contact angle measurement, swelling degree measurement and complete dissolution time control after impregnation in the model lotion, and heat seal strength measurement at 165°C to ensure the performance of the water-soluble film.

Benefits of technology

It realizes the sealing strength of the drug packaging body during long-term storage and transportation, prevents damage to the heat sealing area, and ensures the safety and appearance quality of the drug.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004200941370000041
    Figure BDA0004200941370000041
  • Figure BDA0004200941370000231
    Figure BDA0004200941370000231
  • Figure HDA0004200941380000011
    Figure HDA0004200941380000011
Patent Text Reader

Abstract

Provided are a water-soluble film that maintains good water solubility and is less likely to have a reduced seal strength during long-term storage when packaging a detergent or other pharmaceutical product, a method for producing the same, and a package obtained by packaging a pharmaceutical product using the water-soluble film. The water-soluble film contains polyvinyl alcohol having a polymerization degree of 100 to 3000 and 1 to 50 parts by mass of a polyol-based plasticizer relative to 100 parts by mass of the polyvinyl alcohol, wherein after the water-soluble film is immersed in a model detergent for 24 hours, when deionized water is dripped onto the surface of the film, the contact angle after 6 seconds of dripping is 20 to 35°, after the water-soluble film is immersed in a model detergent for 24 hours, when it is immersed in deionized water at 5°C, the complete dissolution time is within 100 seconds, and the swelling degree of the water-soluble film when immersed in the model detergent for 1 hour is 30 to 50%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a water-soluble film composed of polyvinyl alcohol which is suitable for use in packaging of various medicines, etc., as well as a method for producing the water-soluble film and a package using the same. Background Art

[0002] Water-soluble films are widely used in packaging of various drugs such as liquid detergents and pesticides, seed tapes containing seeds, etc., due to their excellent solubility in water. Polyvinyl alcohol (hereinafter sometimes referred to as PVA) is mainly used as the water-soluble film used in such applications. It is also known that the water solubility of the water-soluble film can be improved by adding various additives such as plasticizers to the water-soluble film containing polyvinyl alcohol, or by using modified polyvinyl alcohol introduced with a carboxyl group as the raw material of the water-soluble film.

[0003] In recent years, among these uses, the use of packaging bodies made of household detergents and other medicines with water-soluble films has become widely popular. Generally, when manufacturing such packaging bodies, the ends of the water-soluble film are heat-sealed to each other so that the water-soluble film is subjected to tension and the medicine is packaged, thereby suppressing wrinkles in the packaging body and making the appearance look good. However, if the packaging body in such a tensioned state is stored for a long time, there is a problem that the tension of the packaging body is lost over time and the appearance becomes poor.

[0004] In order to solve this problem, Patent Document 1 proposes a water-soluble film containing a PVA-based resin and a plasticizer, wherein the area change rate of the water-soluble film when immersed in a predetermined solution shows a specific value. It is claimed that the water-soluble film can be used without impairing the water solubility of the water-soluble film, and can obtain a water-soluble film that can form a good package without impairing the tension of the water-soluble film over time even when a liquid such as a liquid detergent is packaged into a package.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Application WO2017 / 043505 Publication Summary of the invention

[0008] Problems to be solved by the invention

[0009] However, it is known that in recent years, even if the package is obtained by using the water-soluble film described in Patent Document 1, the sealing strength of the heat-sealed portion may be reduced or the heat-sealed portion may be damaged when the package is stored for a long time, such as by using a container for long-term sea transportation. This problem is more obvious in a package obtained by heat-sealing the water-soluble film under tension in order to make the appearance of the package look good. In addition, it is more likely to be manifested significantly due to the thinning of water-soluble films accompanied by environmental problems in recent years.

[0010] The main component of the medicine packaged with the water-soluble film is a surfactant, among which there are many substances with low molecular weight and high polarity. In addition, the PVA contained in the water-soluble film is a hydrophilic polymer, and has high affinity with these highly polar substances. Therefore, it can be inferred that if the package obtained by using this water-soluble film is stored for a long time, these substances will penetrate into the water-soluble film and reach the heat-sealed portion, causing adverse effects on the sealing strength.

[0011] The object of the present invention is to provide a water-soluble film which maintains good water solubility and is less likely to cause a decrease in sealing strength during long-term storage when packaging a drug such as a detergent, a method for producing the same, and a package obtained by packaging a drug using the water-soluble film.

[0012] Means used to solve problems

[0013] The present inventors have conducted intensive research and found that the above-mentioned problems can be solved by setting the contact angle when a model detergent is added dropwise to a water-soluble film, the complete dissolution time when the film is immersed in the model detergent and then immersed in deionized water, and the swelling degree when immersed in the model detergent to specific ranges. Based on this finding, the inventors have conducted further research and completed the present invention.

[0014] That is, the present invention relates to:

[0015] [1] A water-soluble film comprising PVA having a degree of polymerization of 100 to 3,000 and containing 1 to 50 parts by mass of a polyol plasticizer per 100 parts by mass, after the water-soluble film is immersed in a model detergent containing 8.6% by mass of monoethanolamine, 23.8% by mass of dodecylbenzenesulfonic acid, 9.5% by mass of propylene glycol, 23.8% by mass of lauryl alcohol ethoxylate-7-ethylene oxide adduct, 19.1% by mass of oleic acid, 9.5% by mass of diethylene glycol and 5.7% by mass of water at 23°C and 50% RH for 24 hours, the contact angle of deionized water dropped onto the film surface after 6 seconds of dropping is 20° or more, after the water-soluble film is immersed in the model detergent at 23°C and 50% RH for 24 hours, the complete dissolution time when immersed in deionized water at 5°C is within 100 seconds, and the swelling degree of the water-soluble film when immersed in the model detergent at 23°C and 50% RH for 1 hour is 30 to 50%.

[0016] Furthermore, the present invention relates to:

[0017] [2] The water-soluble film according to [1], wherein after the water-soluble film is immersed in the model detergent at 23°C and 50% RH for 24 hours, the contact angle of deionized water dropped onto the film surface 6 seconds after the drop is 35° or less;

[0018] [3] The water-soluble film according to [1] or [2], wherein the water-soluble film is immersed in the model detergent at 23°C and 50% RH for 24 hours and then heat-sealed at 165°C, and the seal strength is 2.0 to 10.0 N / 15 mm;

[0019] [4] The water-soluble film according to any one of [1] to [3] above, wherein the PVA is a carboxylic acid-modified or sulfonic acid-modified PVA having a saponification degree of 85 mol % or more;

[0020] [5] The water-soluble film according to any one of [1] to [4] above, which has a thickness of 5 to 80 μm;

[0021] [6] A method for producing a water-soluble film, which is a method for producing a water-soluble film according to any one of [1] to [5], wherein a film-forming stock solution containing PVA is cast in a film form on a support through a die lip from a mold and dried, wherein the draft ratio obtained by dividing the linear velocity of the support on which the film-forming stock solution is cast by the linear velocity of the film-forming stock solution in the die lip is 2 to 60, and the rate of decrease of the volatile components of the film-forming stock solution on the support is 0.5 to 7% by mass / second;

[0022] [7] The method for producing a water-soluble film according to [6] above, wherein the stretch ratio obtained by dividing the linear velocity of the support on which the film-forming stock solution is cast by the winding velocity of the dried film is 0.95 to 1.8;

[0023] [8] The method for producing a water-soluble film according to [6] or [7], comprising: heat-treating the water-soluble film at 80 to 300° C.;

[0024] [9] A package, wherein the water-soluble film according to any one of [1] to [5] contains a drug;

[0025]

[10] The package according to [9] above, wherein the chemical is a pesticide, a detergent or a disinfectant;

[0026]

[11] The package according to [9] or

[10] above, wherein the drug is in liquid form.

[0027] Effects of the Invention

[0028] According to the present invention, there are provided a water-soluble film which maintains good water solubility and is less likely to cause a decrease in seal strength during long-term storage when packaging a drug such as a detergent, a method for producing the same, and a package obtained by packaging a drug using the water-soluble film. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a diagram for explaining a method for measuring the seal strength when a water-soluble film is immersed in a model detergent under an environment of 23°C and 50% RH for 24 hours and then heat-sealed at 165°C. DETAILED DESCRIPTION

[0030] Hereinafter, the present invention will be described in detail.

[0031] <Model Wash>

[0032] In the present invention, the model detergent simulating a household detergent is a detergent having the following composition.

[0033]

[0034] <Contact Angle of Water-Soluble Film>

[0035] In the present invention, after the water-soluble film is immersed in a model detergent at 23°C and 50% RH for 24 hours, the contact angle (hereinafter sometimes referred to as the contact angle) 6 seconds after deionized water is dropped onto the surface of the film is measured using the following method: <1> ~ <4> The method was used for determination.

[0036] <1> The water-soluble film was stored in a room at 23° C. and 50% RH for 16 hours or more to adjust the humidity.

[0037] <2> The water-soluble film having been conditioned in humidity was immersed in a model detergent having a mass 100 times or more of the film under an environment of 23° C. and 50% RH for 24 hours.

[0038] <3> The water-soluble film is taken out from the model detergent, and the model detergent attached to the surface of the water-soluble film is wiped off with filter paper. Then, the change in contact angle over time when deionized water droplets are added to the surface of the water-soluble film is continuously recorded using the following apparatus / conditions, and the contact angle 6 seconds after the addition is calculated based on the graph.

[0039] Device: Mobile Surface Analyzer manufactured by KRUSS

[0040] Syringe Dosing System from (Kruss Item#MSA)

[0041] (Kruss Item #DS3910)

[0042] Measurement environment: 23°C, 35% RH

[0043] Determination steps:

[0044] Test piece size: 2 inches x 3 inches

[0045] Deionized water drop volume: 1μL

[0046] The contact time between the droplet and the membrane was set to 0 seconds.

[0047] Time measurement up to 10 seconds (0.06 second intervals)

[0048] The Young-Laplace method was used to fit the droplet contact angle.

[0049] <4> This measurement was repeated three times, and the average value thereof was used as the contact angle after immersion in the detergent.

[0050] It should be noted that the reason for selecting the data after 6 seconds of dropping is that the data after about 6 seconds of dropping has the smallest deviation and can obtain a measured value with good accuracy.

[0051] In the present invention, the contact angle of the water-soluble film is more than 20 °. When the contact angle of the water-soluble film is less than 20 °, the sealing strength (hereinafter sometimes referred to as sealing strength) during long-term storage when the detergent and other medicaments are packaged is likely to become insufficient. The lower limit of the contact angle of the water-soluble film is preferably more than 22 °, more preferably more than 23 °, and further preferably more than 24 °. On the other hand, the upper limit of the contact angle of the water-soluble film is preferably less than 35 °, more preferably less than 33 °, further preferably less than 31 °, and particularly preferably less than 29 °. By making the contact angle of the water-soluble film below the above upper limit, the sealing strength easily becomes sufficient.

[0052] It can be inferred that the contact angle of the water-soluble film depends significantly on the affinity between the water-soluble film and the model lotion on the surface of the water-soluble film. Therefore, the contact angle of the water-soluble film can be controlled by adjusting the composition of the water-soluble film (e.g., saponification degree, modification degree, type and content of plasticizer, additives of PVA) and film-making conditions (draw-down ratio, drying conditions, stretching ratio, etc.) that affect the hydrophilicity of the surface of the water-soluble film.

[0053] <Swelling degree of water-soluble film>

[0054] In the present invention, the swelling degree of the water-soluble film (hereinafter sometimes referred to as swelling degree) when the water-soluble film is immersed in a model detergent at 23° C. and 50% RH for 1 hour is measured using the following method: <1> ~ <4> The method was used for determination.

[0055] <1> A test piece measuring 20 cm in the width direction×20 cm in the length direction was cut out from the water-soluble film.

[0056] <2> The cut test piece was stored in a room at 23° C. and 50% RH for 16 hours or more to adjust the humidity.

[0057] <3> The mass of the humidified test piece was measured as "mass of the test piece before immersion in the model detergent", and the test piece was immersed in a model detergent of 100 times or more the mass of the test piece at 23°C and 50% RH for 1 hour.

[0058] <4> The test piece was taken out from the model detergent, and the model detergent attached to the surface of the water-soluble film was wiped off with filter paper. Then, the mass of the test piece was measured under an environment of 23°C and 50% RH as "mass of the test piece after immersion in the model detergent". The swelling degree of the water-soluble film was calculated using the following formula.

[0059] Swelling degree of water-soluble film (%) = {(mass of test piece after immersion in model detergent - mass of test piece before immersion in model detergent) / mass of test piece before immersion in model detergent} × 100

[0060] In the present invention, the swelling degree of the water-soluble film is 30 to 50%. When the swelling degree of the water-soluble film exceeds 50%, the sealing strength may become insufficient by allowing the water-soluble film to absorb the model lotion. The upper limit of the swelling degree of the water-soluble film is preferably 45% or less, more preferably 43% or less, and further preferably 41% or less. On the other hand, when the swelling degree of the water-soluble film is less than 30%, it is observed that the amount of PVA crystals in the water-soluble film increases, so it can be inferred that the softening of the water-soluble film during heat sealing becomes insufficient and the sealing strength becomes insufficient. The lower limit of the swelling degree of the water-soluble film is preferably 32% or more, more preferably 34% or more, and further preferably 36% or more.

[0061] It can be inferred that the swelling degree of the water-soluble film is significantly affected by the PVA crystal structure such as PVA crystal and PVA amorphous in the water-soluble film. Therefore, the swelling degree of the water-soluble film can be controlled by adjusting the composition of the water-soluble film (for example, the saponification degree of PVA, the degree of modification, the type and content of the plasticizer) and the film-making conditions (draw-down ratio, drying conditions, stretching ratio, etc.).

[0062] <Complete dissolution time of water-soluble film>

[0063] In the present invention, the complete dissolution time (hereinafter sometimes referred to as the complete dissolution time) when the water-soluble film is immersed in a model detergent at 23°C and 50% RH for 24 hours and then immersed in deionized water at 5°C is calculated using the following method: <1> ~ <6> The method was used for determination.

[0064] <1> The water-soluble film was placed in a constant temperature and humidity chamber adjusted to 20° C. and 65% RH for 16 hours or more to adjust the humidity.

[0065] <2> A rectangular sample of 40 mm in length and 35 mm in width was cut out from the moisture-conditioned water-soluble film and immersed in a model detergent of 100 times or more the mass of the film under an environment of 23° C. and 50% RH for 24 hours.

[0066] <3> 300 mL of deionized water was placed in a 500 mL beaker, and the mixture was stirred at 280 rpm using a magnetic stirrer equipped with a 3 cm long rod, and the water temperature was adjusted to 5+0.3°C.

[0067] <4> The membrane sample was taken out from the model lotion, and after quickly wiping off the model lotion attached to the surface with filter paper, it was clamped and fixed between two plastic plates of 50 mm × 50 mm with an opening of a rectangular window (hole) of 35 mm in length × 23 mm in width, in such a way that the length direction of the sample was parallel to the length direction of the window and the sample was located approximately in the center of the width direction of the window.

[0068] <5> Be careful not to <4> The sample fixed on the plastic plate was immersed in deionized water in a beaker while touching the bar of the magnetic stirrer.

[0069] <6> The time from immersion in deionized water to complete disappearance of the sample immersed in deionized water was measured.

[0070] It should be noted that, in the present invention, “the sample completely disappears” means that no dissolved residue of the water-soluble film that can be visually identified is observed.

[0071] In the present invention, the complete dissolution time of the water-soluble film is within 100 seconds. If the complete dissolution time exceeds 100 seconds, it is sometimes difficult to be used for the packaging of various medicaments such as liquid detergents and pesticides. The upper limit of the complete dissolution time is preferably within 90 seconds, more preferably within 75 seconds, and more preferably within 60 seconds. On the other hand, the lower limit of the complete dissolution time of the water-soluble film is not particularly limited. If the complete dissolution time is too short, there is a tendency that the water-soluble film absorbs moisture in the air and causes the water-soluble film to adhere to each other, or the strength of the water-soluble film is easily reduced. The lower limit of the complete dissolution time is preferably more than 5 seconds, more preferably more than 10 seconds, more preferably more than 15 seconds, and particularly preferably more than 20 seconds.

[0072] It can be inferred that the complete dissolution time of the water-soluble film is strongly affected by the affinity of PVA to water and the PVA crystal structure such as PVA crystal and PVA amorphous in the water-soluble film. Therefore, by adjusting the composition of the water-soluble film (for example, the saponification degree of PVA, the degree of modification, the type and content of the plasticizer) and the film-making conditions (draw-down ratio, drying conditions, stretching ratio, etc.), the complete dissolution time of the water-soluble film can be controlled.

[0073] <165°C Seal Strength of Water-Soluble Film>

[0074] In the present invention, the seal strength when the water-soluble film is immersed in a model detergent at 23°C and 50% RH for 24 hours and then heat-sealed at 165°C (hereinafter sometimes referred to as 165°C seal strength) is measured by the following method: <1> ~ <6> The method was used for determination. Figure 1 This is a diagram for explaining the method of measuring the seal strength at 165°C. Figure 1 (a) is a view of the water-soluble film observed from the thickness direction. Figure 1 (b) is in the following <5> FIG. 7 is a diagram showing the water-soluble film when it is set on the chuck and viewed from the side.

[0075] <1> like Figure 1 As shown in (a) of FIG. 1 , ten or more test pieces each having a width direction of 100 mm and a length direction of 15 mm were cut out from the water-soluble film.

[0076] <2> The cut test piece was stored in a room at 23° C. and 50% RH for 16 hours or more to adjust the humidity.

[0077] <3> The humidity-conditioned test pieces were immersed in a model detergent of 100 times or more the mass of the test pieces for 1 hour under an environment of 23° C. and 50% RH so that the test pieces did not overlap.

[0078] <4> Take the test piece out of the model lotion and wipe off the model lotion attached to the surface of the water-soluble film with filter paper. Figure 1 As shown in (b), two test pieces were overlapped and heat-sealed at 23°C and 50% RH using a heat tilting device HG-100-2 manufactured by Toyo Seiki Seisaku-sho Co., Ltd., with a heat sealing pressure of 1.2 MPa, with one short side of 15 mm long being heat-sealed at a width of 5 mm. Five or more sets of heat-sealed test pieces were prepared.

[0079] <5> The short side of the heat-sealed test piece of the heat-sealed group was peeled off. Figure 1 As shown in (b) of FIG. 1 , each test piece was attached to the chuck of a table-type precision universal testing machine AGS-H manufactured by Shimadzu Corporation, and the maximum test force when stretched under the following conditions was measured.

[0080] Atmosphere: 23°C, 50% RH

[0081] Chuck spacing: 50mm

[0082] Stretching speed: 300mm / min

[0083] <6> This measurement is performed on 5 or more sets of heat-sealed test pieces, and the average value of the obtained maximum test forces is defined as the 165° C. seal strength [N / 15 mm].

[0084] In the present invention, the 165°C seal strength of the water-soluble film is preferably 2.0 to 10.0 N / 15 mm. By setting the 165°C seal strength to 2.0 N / 15 mm or more, the sealed portion of the package containing the medicine is not easily damaged during transportation. The 165°C seal strength is more preferably 2.5 N / 15 mm or more, and further preferably 3.0 N / 15 mm or more. On the other hand, by setting the 165°C seal strength to 10.0 N / 15 mm or less, the strength of the water-soluble film is prevented from being reduced, and the water-soluble film other than the heat-sealed portion is not easily damaged. The 165°C seal strength is more preferably 9.5 N / 15 mm or less, and further preferably 8.5 N / 15 mm or less.

[0085] <Thickness of water-soluble film>

[0086] The upper limit of the thickness of the water-soluble film of the present invention is preferably 80 μm or less, more preferably 70 μm or less, further preferably 60 μm or less, and particularly preferably 50 μm or less. On the other hand, the lower limit of the thickness of the water-soluble film is preferably 5 μm or more, more preferably 10 μm or more, further preferably 15 μm or more, and particularly preferably 20 μm or more. By making the thickness of the water-soluble film above the above lower limit, it is not easy to open holes when the water-soluble film is made into a package. It should be noted that the thickness of the water-soluble film can be obtained by measuring the thickness of any 10 places (for example, any 10 places on a straight line drawn along the length direction of the water-soluble film) and taking the form of their average value.

[0087] <pva>

[0088] The water-soluble film of the present invention contains PVA. As PVA, PVA produced by saponifying a vinyl ester polymer obtained by polymerizing a vinyl ester monomer can be used. As the vinyl ester monomer, for example, vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl laurate, vinyl stearate, vinyl benzoate, vinyl pivalate, vinyl versatate, etc. can be listed, and among these, vinyl acetate is preferred.

[0089] The vinyl ester polymer is preferably obtained using only one or two or more vinyl ester monomers as monomers, more preferably only one vinyl ester monomer as a monomer, and may be a copolymer of one or two or more vinyl ester monomers and other monomers copolymerizable therewith.

[0090] Examples of such other monomers copolymerizable with the vinyl ester monomer include ethylene; olefins having 3 to 30 carbon atoms such as propylene, 1-butene, and isobutylene; acrylic acid or its salts; acrylic acid esters such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, dodecyl acrylate, and octadecyl acrylate; methacrylic acid or its salts; methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, 2-ethylhexyl methacrylate, dodecyl methacrylate, and octadecyl methacrylate; acrylamide, N-methylacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, diacetoneacrylamide, acrylamidopropanesulfonic acid or its salts, acrylamidopropyldimethylamine or its salts, N-hydroxymethyl acrylamide derivatives such as acrylamide or its derivatives; methacrylamide derivatives such as methacrylamide, N-methylmethacrylamide, N-ethylmethacrylamide, methacrylamidepropanesulfonic acid or its salts, methacrylamidopropyldimethylamine or its salts, N-hydroxymethylmethacrylamide or its derivatives; N-vinylamides such as N-vinylformamide, N-vinylacetamide, and N-vinylpyrrolidone; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, tert-butyl vinyl ether, dodecyl vinyl ether, and stearyl vinyl ether; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl halides such as vinyl chloride, vinylidene chloride, vinyl fluoride, and vinylidene fluoride; allyl compounds such as allyl acetate and allyl chloride; maleic acid or its salts, esters, or anhydrides; itaconic acid or its salts, esters, or anhydrides; vinyl silyl compounds such as vinyltrimethoxysilane; isopropenyl acetate, etc. The vinyl ester polymer may have structural units derived from one or two or more of these other monomers.

[0091] Among these other monomers that can be copolymerized with the vinyl ester monomer, in the case of monomers that produce bulky functional groups in the polymer side chains after polymerization and saponification, it is easy to reduce the sealing strength of the resulting water-soluble film, so it is not preferred. From this point of view, olefins with a small number of carbon atoms such as ethylene and propylene; carboxylic acid monomers such as acrylic acid and methacrylic acid; sulfonic acid monomers are preferred. Among these, from the perspective of easily showing a balance in the contact angle, swelling degree and complete dissolution time of the resulting water-soluble film, carboxylic acid monomers or sulfonic acid monomers are more preferred.

[0092] The PVA contained in the water-soluble film of the present invention is preferably a carboxylic acid-modified PVA obtained by saponifying a carboxylic acid-vinyl acetate copolymer obtained by copolymerizing vinyl acetate and a carboxylic acid-based monomer. The upper limit of the degree of modification of the carboxylic acid-modified PVA is preferably 10 mol% or less, more preferably 8 mol% or less, and further preferably 6 mol% or less. On the other hand, the lower limit of the degree of modification of the carboxylic acid-modified PVA is preferably 0.5 mol% or more, more preferably 1 mol% or more, and further preferably 2 mol% or more.

[0093] The PVA contained in the water-soluble film of the present invention is also preferably a sulfonic acid-modified PVA obtained by saponifying a sulfonic acid-vinyl acetate copolymer obtained by copolymerizing vinyl acetate and a sulfonic acid-based monomer. The upper limit of the degree of modification of the sulfonic acid-modified PVA is preferably 8 mol% or less, more preferably 6 mol% or less, and further preferably 4 mol% or less. On the other hand, the lower limit of the degree of modification of the sulfonic acid-modified PVA is preferably 0.3 mol% or more, more preferably 0.7 mol% or more, and further preferably 1 mol% or more.

[0094] From the viewpoint of water solubility of the water-soluble film and suppression of pore opening, the upper limit of the proportion of structural units derived from other monomers in the vinyl ester polymer is preferably 15 mol% or less, more preferably 5 mol% or less, based on the number of moles of all structural units constituting the vinyl ester polymer.

[0095] In the present invention, the degree of polymerization of PVA contained in the water-soluble film is 100 to 3000. When the degree of polymerization of PVA is less than 100, the strength of the water-soluble film sometimes becomes insufficient. The degree of polymerization of PVA is preferably 200 or more, more preferably 300 or more, and further preferably 500 or more. On the other hand, when the degree of polymerization of PVA exceeds 3000, it is sometimes difficult to ensure the productivity of PVA and the water-soluble film and the water solubility of the water-soluble film. The degree of polymerization of PVA is preferably 2500 or less, more preferably 2000 or less, and further preferably 1500 or less. Here, the degree of polymerization refers to the average degree of polymerization (Po) measured in accordance with the description of JIS K6726-1994, which can be obtained by the following formula based on the intrinsic viscosity [η] (dl / g) measured in water at 30°C after re-saponifying and refining the PVA.

[0096] Po=([η]×10 4 / 8.29) (1 / 0.62)

[0097] In the present invention, the saponification degree of PVA contained in the water-soluble film is preferably 80 to 99.5 mol%. Here, the saponification degree of PVA refers to the ratio (mol %) of the molar number of the vinyl alcohol unit relative to the total molar number of the structural unit (typically, a vinyl ester monomer unit) and the vinyl alcohol unit in the PVA that can be converted into the vinyl alcohol unit by saponification. The saponification degree of PVA can be measured according to the description of JIS K6726-1994.

[0098] Among PVA, in the case of unmodified PVA and hydrophobic ethylene-modified PVA, the higher the saponification degree, the fewer the acetic acid groups that disturb the PVA crystal structure in the water-soluble film become, so the lotion is not easy to penetrate, and its influence is reduced. If the saponification degree is too high, the water solubility of the water-soluble film is likely to decrease. From this viewpoint, the upper limit of the saponification degree of unmodified PVA and ethylene-modified PVA is preferably below 99.5 mol%, more preferably below 97 mol%, further preferably below 95 mol%, and particularly preferably below 93 mol%. On the other hand, the lower limit of the saponification degree of unmodified PVA and hydrophobic ethylene-modified PVA is preferably above 80 mol%, more preferably above 83 mol%, further preferably above 85 mol%, and particularly preferably above 87 mol%. By making the saponification degree of unmodified PVA and hydrophobic ethylene-modified PVA above the above lower limit, the strength of the water-soluble film is easily sufficient. It should be noted that unmodified PVA refers to PVA obtained by saponifying a vinyl acetate homopolymer obtained by homopolymerizing vinyl acetate, and ethylene-modified PVA refers to PVA obtained by saponifying an ethylene-vinyl acetate copolymer obtained by copolymerizing vinyl acetate and ethylene.

[0099] Among PVA, in the case of carboxylic acid-modified PVA and sulfonic acid-modified PVA, since the introduced carboxyl group and sulfonic group are hydrophilic groups, even if the saponification degree is increased, the water solubility of the water-soluble film becomes good. The upper limit of the saponification degree of carboxylic acid-modified PVA and sulfonic acid-modified PVA is preferably 99 mol% or less, more preferably 97 mol% or less, and particularly preferably 96 mol% or less. On the other hand, the lower limit of the saponification degree of carboxylic acid-modified PVA and sulfonic acid-modified PVA is preferably 85 mol% or more, more preferably 90 mol% or more, and further preferably 93 mol% or more.

[0100] In the water-soluble film of the present invention, as PVA, one type of PVA may be used alone, or two or more types of PVAs having different polymerization degrees, saponification degrees, modification degrees, etc. may be used as a blend.

[0101] In the present invention, the upper limit of the content of PVA in the water-soluble film is not particularly limited, but the lower limit of the content of PVA is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 85% by mass or more.

[0102] <Polyol plasticizer>

[0103] In the present invention, the water-soluble film contains 1 to 50 parts by mass of a polyol plasticizer relative to 100 parts by mass of PVA. When the content of the polyol plasticizer exceeds 50 parts by mass, there is a tendency for the contact angle and swelling degree of the resulting water-soluble film to become too large. The upper limit of the content of the polyol plasticizer is preferably 40 parts by mass or less, more preferably 30 parts by mass or less. On the other hand, when the content of the polyol plasticizer is less than 1 part by mass, there is a tendency for the contact angle of the resulting water-soluble film to become too small or the swelling degree to become too large. In addition, there is a tendency for the 165°C sealing strength of the resulting water-soluble film to become too low. The lower limit of the content of the polyol plasticizer is preferably 3 parts by mass or more, more preferably 5 parts by mass or more.

[0104] In the present invention, as the polyol plasticizer contained in the water-soluble film, for example, ethylene glycol, glycerine, diglycerine, propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, trimethylolpropane, sorbitol etc. can be listed. These polyol plasticizers can be used alone or in combination. Among these polyol plasticizers, from the viewpoint of being particularly easy to adjust the contact angle of the water-soluble film, ethylene glycol or glycerine is preferably used, and glycerine is more preferably used. It should be noted that by making the film-making stock solution of the water-soluble film contain the polyol plasticizer, the obtained water-soluble film can be made to contain the polyol plasticizer. In addition, the ratio of the content of the polyol plasticizer in the water-soluble film is substantially equal to the ratio of the addition amount of the polyol plasticizer in the film-making stock solution of the water-soluble film.

[0105] The type / amount of the polyol plasticizer contained in the film-making stock solution of the water-soluble film affects the PVA crystal structure in the water-soluble film. If the amount of the polyol plasticizer with high affinity to PVA is appropriately increased, when the PVA film obtained by casting the film-making stock solution described later on the support is dried, the mobility of the PVA molecules will increase, and thus, when the water-soluble film is manufactured, the crystallization rate of PVA becomes faster, and the crystallization of PVA is easily generated in the obtained water-soluble film. On the other hand, if the amount of the polyol plasticizer is excessively increased, the interaction between the PVA polyol system-plasticizer is enhanced, and the interaction between the PVA molecules is reduced, and thus it is not easy to generate the crystallization of PVA in the obtained water-soluble film. It can be inferred here that the swelling degree of the water-soluble film depends on the amount of PVA crystals in the water-soluble film. In addition, the surface of the water-soluble film that becomes the interface with the hydrophobic air also has a tendency to be hydrophobic, but the slower the crystallization rate of the PVA when the water-soluble film is manufactured, the stronger this tendency is. Therefore, by adjusting the type and amount of the polyol plasticizer, the contact angle and swelling degree of the water-soluble film can be adjusted.

[0106] <Starch / Water-soluble polymer>

[0107] The water-soluble film of the present invention may contain a water-soluble polymer other than starch and / or PVA for the purpose of imparting mechanical strength to the water-soluble film or maintaining the handleability of the water-soluble film.

[0108] Examples of starch include natural starches such as corn starch, potato starch, sweet potato starch, wheat starch, rice starch, tapioca starch, and sago starch; and processed starches that have been subjected to etherification, esterification, oxidation, and the like. Processed starches are more preferred.

[0109] The upper limit of the starch content in the water-soluble film is preferably 15 parts by mass or less, more preferably 10 parts by mass or less relative to 100 parts by mass of PVA. By making the starch content below the upper limit, it is easy to prevent the process quality from deteriorating when manufacturing the water-soluble film.

[0110] Examples of water-soluble polymers other than PVA include dextrin, gelatin, glue, casein, shellac, gum arabic, polyacrylamide, sodium polyacrylate, polyvinyl methyl ether, a copolymer of methyl vinyl ether and maleic anhydride, a copolymer of vinyl acetate and itaconic acid, polyvinyl pyrrolidone, cellulose, acetyl cellulose, acetyl butyl cellulose, carboxymethyl cellulose, methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, sodium alginate, and the like.

[0111] The upper limit of the content of water-soluble polymers other than PVA in the water-soluble film is preferably 15 parts by mass or less, more preferably 10 parts by mass or less relative to 100 parts by mass of PVA. By making the content of the water-soluble polymer below the upper limit, it is easy to prevent the water solubility of the water-soluble film from being impaired.

[0112] <Surfactant>

[0113] In the present invention, the water-soluble film preferably contains a surfactant from the viewpoint of improving its handling properties or peeling properties on a self-made membrane device when manufacturing the water-soluble film. The type of surfactant is not particularly limited, and examples thereof include anionic surfactants, nonionic surfactants, and the like.

[0114] Examples of the anionic surfactant include carboxylic acid type surfactants such as potassium laurate; sulfate ester type surfactants such as octyl sulfate; and sulfonic acid type surfactants such as dodecylbenzenesulfonate.

[0115] Examples of the nonionic surfactant include alkyl ether types such as polyoxyethylene lauryl ether and polyoxyethylene oleyl ether; alkyl phenyl ether types such as polyoxyethylene octylphenyl ether; alkyl ester types such as polyoxyethylene laurate; alkyl amine types such as polyoxyethylene lauryl amino ether; alkyl amide types such as polyoxyethylene lauramide; polypropylene glycol ether types such as polyoxyethylene polyoxypropylene ether; alkanolamide types such as lauric acid diethanolamide and oleic acid diethanolamide; allyl phenyl ether types such as polyoxyalkylene allyl phenyl ether, and the like.

[0116] The surfactant may be used alone or in combination of two or more. Among these surfactants, nonionic surfactants are preferred, alkanolamide-type surfactants are more preferred, and dialkanolamides (e.g., diethanolamide, etc.) of aliphatic carboxylic acids (e.g., saturated or unsaturated aliphatic carboxylic acids having 8 to 30 carbon atoms, etc.) are further preferred, in order to further reduce the abnormality of the film surface when the water-soluble film is manufactured.

[0117] The upper limit of the content of the surfactant in the water-soluble film is preferably less than 10 mass parts, more preferably less than 1 mass part, more preferably less than 0.5 mass part, and particularly preferably less than 0.3 mass part relative to 100 mass parts of PVA. By making the content of the surfactant below the above upper limit, it is easy to prevent the surfactant from oozing out of the surface of the water-soluble film, or the appearance of the water-soluble film is deteriorated due to the aggregation of the surfactant. On the other hand, the lower limit of the content of the surfactant is preferably more than 0.01 mass part, more preferably more than 0.02 mass part, and more preferably more than 0.05 mass part relative to 100 mass parts of PVA. By making the content of the surfactant be more than the above lower limit, it is easy to improve the peeling property of peeling off on the homemade film device when manufacturing the water-soluble film. In addition, it is easy to prevent adhesion between the water-soluble film.

[0118] <Filling Agent>

[0119] The water-soluble film of the present invention may contain a filler. By containing a filler, the mechanical strength and handling properties of the water-soluble film can be improved, and since the model detergent cannot penetrate the filler, the path length required for penetration in the film becomes longer, and thus improvement in barrier properties can be expected.

[0120] Examples of the filler include carbon black, metal powder, silica, alumina, calcium carbonate, titanium dioxide, talc, mica, and clay minerals such as bentonite.

[0121] The upper limit of the content of the filler in the water-soluble film is preferably 40 parts by mass or less, more preferably 20 parts by mass or less, and further preferably 10 parts by mass or less relative to 100 parts by mass of PVA. By making the content of the filler below the above upper limit, it is easy to prevent the 165°C sealing strength of the water-soluble film from being reduced, or the appearance such as transparency from being deteriorated. The lower limit of the content of the filler in the water-soluble film is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and further preferably 1 parts by mass or more relative to 100 parts by mass of PVA.

[0122] <Other ingredients>

[0123] The water-soluble film of the present invention may contain water, antioxidants, ultraviolet absorbers, lubricants, cross-linking agents, colorants, preservatives, mildew-proofing agents, other polymer compounds and other components in addition to plasticizers, starch, water-soluble polymers other than PVA, and surfactants within the range that does not hinder the effect of the present invention. The total value of the mass of each of PVA, plasticizers, starch, water-soluble polymers other than PVA, and surfactants in the total mass of the water-soluble film of the present invention is preferably in the range of 60 to 100 mass%, more preferably in the range of 80 to 100 mass%, and further preferably in the range of 90 to 100 mass%.

[0124] <Method for producing water-soluble film>

[0125] In the present invention, the method for manufacturing the water-soluble film is not particularly limited, and film-making can be performed by any of the following methods: using a film-making stock solution obtained by adding a solvent, an additive, etc. to PVA and homogenizing it, a method for film-making using a cast film method, a wet film method (spraying into a poor solvent), a dry-wet film method, a gel film method (a method of temporarily cooling and gelling the film-making stock solution, extracting and removing the solvent to obtain a water-soluble film), or a combination thereof; a melt extrusion film-making method in which a film-making stock solution is obtained by extruding it from a T die, etc.; an inflation molding method, etc. Among these, a cast film method or a melt extrusion film method is preferably used from the aspect of being able to obtain a uniform water-soluble film with good productivity. Below, the cast film method or the melt extrusion film method for a water-soluble film is described.

[0126] When a water-soluble film is produced by a cast film method or a melt extrusion film method, the film-forming stock solution is heated, the solvent is removed, and the film is solidified. The solidified film is peeled off from the support, dried by a drying roller, a drying furnace, etc. as needed, and further heat-treated as needed and wound up, thereby obtaining a long water-soluble film in a roll shape.

[0127] The upper limit of the volatility of the film-forming stock solution (the concentration of volatile components such as solvents that are removed by volatilization or evaporation during film-forming) is preferably 90% by mass or less, and more preferably 80% by mass or less. By making the volatility of the film-forming stock solution below the above upper limit, the viscosity of the film-forming stock solution becomes low, and it is easy to prevent the thickness uniformity of the obtained water-soluble film from being impaired. On the other hand, the lower limit of the volatility of the film-forming stock solution is preferably 50% by mass or more, and more preferably 55% by mass or more. By making the volatility of the film-forming stock solution above the above lower limit, the viscosity of the film-forming stock solution becomes high, and it is easy to prevent the production of the water-soluble film from becoming difficult.

[0128] Here, the "volatile fraction of the membrane-forming stock solution" in this specification refers to the volatile fraction calculated by the following formula.

[0129] Volatile fraction of film-forming stock solution (mass %) = {(Wa-Wb) / Wa} × 100

[0130] (Wa represents the mass (g) of the film-forming stock solution, and Wb represents the mass (g) of the film-forming stock solution when Wa (g) is dried in an electric drying machine at 105°C for 16 hours.)

[0131] The method for adjusting the film-forming stock solution is not particularly limited, and examples thereof include a method of dissolving PVA and additives such as plasticizers and surfactants in a dissolving tank or the like; a method of melt-kneading PVA in a water-containing state with a plasticizer, a surfactant, etc. using a single screw extruder or a twin screw extruder, etc. Among these, a method of dissolving in a dissolving tank or the like or a method of using a twin screw extruder is preferred.

[0132] The adjusted film-forming stock solution is sent to a T-die or the like through a pipe or the like, and is ejected onto a support in the form of a film through a die lip.

[0133] In the method for producing a water-soluble film of the present invention, in which a film-forming stock solution containing PVA is cast from a mold through a die lip in a film-like state on a support and dried, the draft ratio obtained by dividing the linear velocity of the support on which the film-forming stock solution is to be cast by the linear velocity of the film-forming stock solution in the die lip is preferably 2 to 60. The upper limit of the draft ratio is more preferably 50 or less, further preferably 40 or less, and particularly preferably 30 or less. By making the draft ratio below the above upper limit, it is easy to prevent the contact angle of the obtained water-soluble film from becoming too large, or the swelling degree from becoming too small, or the 165°C sealing strength from decreasing. In addition, by making the draft ratio below the above upper limit, it is easy to prevent the thickness of the obtained water-soluble film from becoming uneven, or the water solubility from decreasing, or the complete dissolution time from becoming long. On the other hand, the lower limit of the draft ratio is more preferably 5 or more, further preferably 8 or more, and particularly preferably 10 or more. By making the draft ratio equal to or greater than the above lower limit, it is easy to prevent the contact angle of the obtained water-soluble film from becoming too small, the swelling degree from becoming too large, or the seal strength at 165° C. from decreasing. It should be noted that the linear velocity of the film-forming stock solution in the die lip can be obtained by dividing the volume flow rate of the film-forming stock solution by the area of ​​the die lip opening (die lip width×lip opening).

[0134] The reason why the stretch ratio affects the contact angle, swelling degree and complete dissolution time of the water-soluble film is not yet clear, but it can be considered that: if the stretch ratio becomes higher, the PVA film formed by casting the film-making solution on the support in a film state is stretched between the die lip and the support, thereby causing the mutual entanglement of the PVA molecular chains in the PVA film to be disassembled, facilitating the crystallization of the PVA during drying and easily generating PVA crystals.

[0135] In the method for producing a water-soluble film of the present invention, the rate of decrease of the volatile components of the film-forming stock solution on the support is preferably 0.5 to 7 mass% / second. The upper limit of the rate of decrease of the volatile components of the film-forming stock solution is preferably less than 6 mass% / second, and more preferably less than 5 mass% / second. By making the rate of decrease of the volatile components of the film-forming stock solution below the above upper limit, it is easy to prevent the contact angle of the obtained water-soluble film from becoming too small, or the swelling degree from becoming too large, or the sealing strength at 165°C from decreasing. On the other hand, the lower limit of the rate of decrease of the volatile components of the film-forming stock solution is more preferably 1 mass% / second or more, and further preferably 2 mass% / second or more. By making the rate of decrease of the volatile components of the film-forming stock solution above the above lower limit, it is easy to prevent the contact angle of the obtained water-soluble film from becoming too large, or the swelling degree from becoming too small, or the sealing strength at 165°C from decreasing.

[0136] The rate of decrease of the volatile components of the membrane-forming stock solution on the support can be calculated by the following formula.

[0137] Reduction rate of volatile components in the film-forming solution on the support = (volatile component ratio of the film-forming solution - volatile component ratio of the film immediately after peeling off from the support) / contact time between the film and the support

[0138] The volatile content in the film can be calculated from the mass change before and after the film is dried in an electric drying machine at 105° C. for 16 hours, similarly to the volatile content in the above-mentioned film-forming stock solution.

[0139] The surface temperature of the support on which the film-making stock solution is to be cast is preferably 50 to 110°C. The upper limit of the surface temperature of the support is more preferably 100°C or less, and further preferably 95°C or less. By making the surface temperature of the support below the above upper limit, it is easy to prevent the contact angle of the obtained water-soluble film from becoming too small, or the swelling degree from becoming too large, or the 165°C sealing strength from decreasing. In addition, when the PVA film formed by the film-making stock solution being cast on the support in a film-like state is dried, it is easy to prevent the occurrence of film surface abnormalities such as foaming. On the other hand, the lower limit of the surface temperature of the support is more preferably 60°C or more, and further preferably 65°C or more. By making the surface temperature of the support above the above lower limit, the PVA film is slowly dried, and it is easy to prevent excessive crystallization of the PVA. As a result, it is easy to prevent the contact angle of the obtained water-soluble film from becoming too large, or the swelling degree from becoming too small, or the 165°C sealing strength from decreasing. In addition, it is easy to prevent the water solubility of the obtained water-soluble film from decreasing and the complete dissolution time from becoming longer.

[0140] The PVA film can be heated and dried on the support, and hot air can be evenly blown to the entire area of ​​the non-contact surface side of the PVA film to adjust the drying speed. The upper limit of the temperature of the hot air is preferably below 105°C, and more preferably below 100°C. By making the temperature of the hot air below the above upper limit, it is easy to prevent the contact angle of the obtained water-soluble film from becoming too small, or the swelling degree from becoming too large, or the sealing strength at 165°C from decreasing. On the other hand, the lower limit of the temperature of the hot air is preferably above 75°C, and more preferably above 85°C. By making the temperature of the hot air above the above lower limit, it is easy to prevent the contact angle of the obtained water-soluble film from becoming too large, or the swelling degree from becoming too small, or the sealing strength at 165°C from decreasing. In addition, it is easy to prevent the water solubility of the obtained water-soluble film from decreasing and the complete dissolution time from becoming longer. In addition, the upper limit of the speed of the hot air is preferably below 10m / second, and more preferably below 7m / second. The lower limit of the speed of the hot air is preferably above 1m / second, and more preferably above 3m / second.

[0141] The PVA film formed by casting the film-making stock solution on the support in a film-like manner is preferably dried on the support to a volatility of 5 to 50% by mass, then peeled off and further dried as needed. The drying method is not particularly limited, and methods of contacting with a drying furnace or a drying roller can be cited. When drying it using multiple drying rollers, it is preferred to make one side and the other side of the PVA film contact the drying rollers alternately so that the physical properties of both sides of the resulting water-soluble film are uniform. The number of drying rollers is preferably 3 or more, more preferably 4 or more, and further preferably 5 or more. The number of drying rollers is preferably 30 or less.

[0142] The upper limit of the temperature of the drying furnace and the drying roller is preferably 110°C or less, more preferably 100°C or less, more preferably 90°C or less, and further preferably 85°C or less. By setting the temperature of the drying furnace and the drying roller to be below the upper limit, it is easy to prevent the water solubility of the water-soluble film from being impaired. On the other hand, the lower limit of the temperature of the drying furnace and the drying roller is preferably 40°C or more, more preferably 45°C or more, and further preferably 50°C or more. By setting the temperature of the drying furnace and the drying roller to be above the lower limit, it is easy to prevent the contact angle of the obtained water-soluble film from becoming too large, the swelling degree from becoming too small, or the sealing strength at 165°C from decreasing.

[0143] In the method for producing a water-soluble film of the present invention, the upper limit of the stretch ratio obtained by dividing the linear speed of the support of the film-casting stock solution by the winding speed of the dried film is preferably 1.80 or less, more preferably 1.75 or less, and further preferably 1.70 or less. By making the stretch ratio below the above upper limit, it is easy to prevent the contact angle of the obtained water-soluble film from becoming too large, or the swelling degree from becoming too small, or the sealing strength at 165°C from decreasing. On the other hand, the lower limit of the stretch ratio is preferably 0.95 or more, more preferably 1.00 or more, and further preferably 1.05 or more. By making the stretch ratio above the above lower limit, it is easy to prevent the contact angle of the obtained water-soluble film from becoming too small, or the swelling degree from becoming too large, or the sealing strength at 165°C from decreasing.

[0144] The reason why the stretching ratio affects the contact angle, swelling degree and 165°C sealing strength of the water-soluble film is not clear, but it can be said that the water-soluble film is always under tension along the flow direction (MD direction) of the film during the drying process, and is actually stretched in the MD direction in conjunction with the volume shrinkage associated with the volatilization of the solvent. It can be considered that if the water-soluble film is stretched while containing a large amount of water, the orientation crystallization of the PVA molecules is likely to occur, and PVA crystals are likely to be generated.

[0145] In the method for producing a water-soluble film of the present invention, it is preferred that the step of heat treating the water-soluble film under the conditions of 80 to 300° C. be included. By performing the heat treatment, the contact angle, swelling degree and complete dissolution time of the water-soluble film can be adjusted. The upper limit of the temperature of the heat treatment is more preferably below 280° C., further preferably below 260° C., and particularly preferably below 240° C. By making the temperature of the heat treatment below the above upper limit, it is easy to prevent the contact angle of the water-soluble film from becoming too large, or the swelling degree from becoming too small, or the sealing strength at 165° C. from decreasing. On the other hand, the lower limit of the temperature of the heat treatment is more preferably above 90° C., further preferably above 100° C., and particularly preferably above 105° C. By making the temperature of the heat treatment above the above lower limit, it is easy to prevent the contact angle of the water-soluble film from becoming too small, or the swelling degree from becoming too large, or the sealing strength at 165° C. from decreasing.

[0146] The water-soluble film produced in this manner is further subjected to humidity conditioning, embossing, cutting of both ends (sides) of the film, etc. as necessary, and then wound up into a roll on a cylindrical core.

[0147] The upper limit of the volatility of the water-soluble film finally obtained through a series of treatments is preferably 5% by mass or less, more preferably 4% by mass or less. The lower limit of the volatility of the water-soluble film is preferably 1% by mass or more, more preferably 2% by mass or more.

[0148] <Purpose>

[0149] The water-soluble film of the present invention can be suitably used for various water-soluble film applications. Examples of such water-soluble films include films for drug packaging, base films for hydraulic transfer, base films for embroidery, release films for artificial marble molding, films for seed packaging, and films for waste storage bags. Among these, the water-soluble film of the present invention is preferably used as a film for drug packaging in terms of more significantly exerting the effects of the present invention.

[0150] As the type of medicament when the water-soluble film of the present invention is used as a film for medicament packaging, pesticides, detergents (including bleaching agents), disinfectants, etc. can be listed. The physical properties of the medicament are not particularly limited, and can be acidic, neutral, or alkaline. In addition, the medicament can contain a boron-containing compound. As the form of the medicament, it can be any one of powder, block, gel and liquid. The packaging form is not particularly limited, and it is preferably a form of unit packaging in which the medicament is sub-packaged in unit amounts (preferably sealed packaging). By packaging the medicament with the film of the present invention as a film for medicament packaging, the package of the present invention is obtained.

[0151] Example

[0152] Hereinafter, the present invention will be specifically described by way of examples etc., but the present invention is not limited to the following examples at all.

[0153] (1) Contact angle of water-soluble film

[0154] By the above method, the water-soluble film was immersed in a model detergent at 23° C. and 50% RH for 24 hours, and then deionized water was dropped onto the film surface. The contact angle was determined 6 seconds after the addition.

[0155] (2) Swelling degree of water-soluble film

[0156] The swelling degree of the water-soluble film was measured by the above method when the water-soluble film was immersed in a model detergent under an environment of 23° C. and 50% RH for 1 hour.

[0157] (3) Complete dissolution time of water-soluble film

[0158] By the above method, the complete dissolution time of the water-soluble film was measured when the film was immersed in a model detergent at 23°C and 50% RH for 24 hours and then immersed in deionized water at 5°C.

[0159] (4) Sealing strength of water-soluble film at 165°C

[0160] The seal strength was measured by the above method when the water-soluble film was immersed in a model detergent at 23°C and 50% RH for 24 hours and then heat-sealed at 165°C.

[0161] (5) Transportation test

[0162] Use the following <1> ~ <7> A transportation test of a packaged body obtained by packaging a model lotion with a water-soluble film was carried out by the method of

[0163] <1> Two test pieces of 7 cm×7 cm were cut out from the water-soluble film.

[0164] <2> The two test pieces cut out were stored in a room at 23° C. and 50% RH for 16 hours or more to adjust the humidity.

[0165] <3> Two test pieces having been humidified were immersed in a model detergent under an environment of 23° C. and 50% RH for 16 hours.

[0166] <4> Two test pieces taken out from the model lotion were overlapped after the model lotion adhering to the surface was wiped off with filter paper, and three sides thereof were heat-sealed with a sealing width of 1 cm to prepare a soft bag with one side open.

[0167] <5> Put 20cm of 3 The model lotion is made by adjusting the sealing width so that no wrinkles are generated on the surface of the soft bag and the film is in an unfolded state, and the remaining side is heat-sealed to produce a packaging body for the model lotion.

[0168] <6> 100 of the above-mentioned packages were prepared, placed in a 45L polyethylene bag, and placed in a cardboard box (320×335×325cm). The gap between the polyethylene bag and the cardboard box was filled with cushioning material. The cardboard boxes containing the packages were piled in a truck and transported 10 times between Okayama Prefecture and Tokyo, Japan.

[0169] <7> The packaged bodies after transportation were visually inspected to check the number of damaged packaged bodies.

[0170] <Example 1>

[0171] 100 parts by mass of carboxylic acid-modified PVA (96 mol% saponification degree, 1200 degree of polymerization) modified with 4 mol% of monomethyl maleate (MMM) obtained by saponifying 4 mol% of polyvinyl acetate modified with MMM, 25 parts by mass of glycerol as a polyol plasticizer, 0.2 parts by mass of lauric acid diethanolamide as a surfactant, and water were put into a twin-screw extruder to prepare a film-making stock solution with a volatile fraction of 60% by mass. The film-making stock solution was ejected from a T-die through a die lip at a draft ratio of 11, cast on a metal roll (support) with a surface temperature of 90°C, and dried by blowing hot air of 100°C at a speed of 5 m / sec to the entire surface not in contact with the support. The reduction rate of the volatile components of the film-making stock solution on the support under these conditions was 2.3% by mass / sec. Next, it was peeled off from the support, and dried from the second drying roller to the final drying roller in such a way that one side and the other side of the PVA film contacted each drying roller alternately. The surface temperature of the second drying roller to the final drying roller was 80°C. Next, for two heat treatment rollers with a surface temperature of 110°C, one side and the other side of the PVA film contacted each heat treatment roller alternately for heat treatment, and then wound on a roll core made of vinyl chloride. The stretching ratio from the support to the winding was 1.4. In this way, a water-soluble film (thickness 40μm, length 1200m, width 1m) was obtained.

[0172] The obtained water-soluble film was used to measure the contact angle, swelling degree, complete dissolution time and seal strength at 165° C. Furthermore, a transportation test was conducted on a package body in which a model detergent was packaged using the water-soluble film. The results are shown in Table 1.

[0173] <Examples 2, 3, Comparative Example 1>

[0174] Respectively, in Example 2, the carboxylic acid-modified PVA modified with 4 mol% of MMM (with a saponification degree of 96 mol% and a polymerization degree of 1200) was changed to a sulfonic acid-modified PVA modified with 2 mol% of 2-acrylamide-2-methylpropanesulfonic acid (AMPS) (with a saponification degree of 99 mol% and a polymerization degree of 1200), in Example 3, the carboxylic acid-modified PVA modified with 4 mol% of MMM (with a saponification degree of 96 mol% and a polymerization degree of 1200) was changed to an unmodified PVA (with a saponification degree of 88 mol% and a polymerization degree of 1200), and in Comparative Example 1, the carboxylic acid-modified PVA modified with 4 mol% of MMM (with a saponification degree of 96 mol% and a polymerization degree of 1200) was changed to an unmodified PVA (with a saponification degree of 99 mol% and a polymerization degree of 1200). Except for this, the same operations as in Example 1 were performed to obtain a water-soluble film. The obtained water-soluble film was used to measure the contact angle, swelling degree, complete dissolution time and seal strength at 165° C. Furthermore, a transportation test was conducted on a package body in which a model detergent was packaged using the water-soluble film. The results are shown in Table 1.

[0175] <Example 4>

[0176] The draft ratio between the T die and the support was changed to 31, the surface temperature of the support was changed to 80°C, the temperature of the hot air blown to the entire surface not in contact with the support was changed to 90°C, the surface temperature of the heat treatment roller was changed to 180°C, and the stretch ratio from the support to the winding was changed to 1.8. Except for this, the same operation as in Example 3 was performed to obtain a water-soluble film. The rate of reduction of the volatile components of the film-making stock solution on the support under this condition was 5.9 mass % / second. The obtained water-soluble film was used to measure the contact angle, swelling degree, complete dissolution time and 165°C sealing strength of the water-soluble film. Furthermore, a transportation test of the packaging body obtained by packaging the model lotion with the water-soluble film was carried out. The results are shown in Table 1.

[0177] <Example 5>

[0178] The draft ratio between the T die and the support was changed to 3, the surface temperature of the support was changed to 105°C, the temperature of the hot air blown to the entire surface not in contact with the support was changed to 105°C, and the surface temperature of the heat treatment roller was changed to 180°C. Except for this, the same operation as in Example 3 was performed to obtain a water-soluble film. It should be noted that the rate of reduction of the volatile components of the film-making stock solution on the support under this condition was 6.7% by mass / second. The obtained water-soluble film was used to measure the contact angle, swelling degree, complete dissolution time and 165°C sealing strength of the water-soluble film. Furthermore, a transportation test of the packaging body obtained by packaging the model lotion with the water-soluble film was carried out. The results are shown in Table 1.

[0179] <Example 6>

[0180] The amount of glycerol as a polyol plasticizer was changed to 42 parts by mass relative to 100 parts by mass of PVA. The same operation as in Example 1 was performed to obtain a water-soluble film. The rate of decrease of the volatile components of the film-making stock solution on the support under this condition was 2.4% by mass / second. The contact angle, swelling degree, complete dissolution time and sealing strength at 165°C of the water-soluble film were measured using the obtained water-soluble film. Furthermore, a transportation test of a package obtained by packaging a model detergent with the water-soluble film was carried out. The results are shown in Table 1.

[0181] <Comparative Example 2>

[0182] The same operation as in Example 3 was performed except that the draft ratio between the T die and the support was changed to 1.2 and the stretch ratio from the support to the winding was changed to 0.8 to obtain a water-soluble film. The contact angle, swelling degree, complete dissolution time and sealing strength at 165° C. of the obtained water-soluble film were measured. Furthermore, a transportation test of a package obtained by packaging a model detergent with the water-soluble film was conducted. The results are shown in Table 1.

[0183] <Comparative Example 3>

[0184] The amount of glycerol as a polyol plasticizer was changed to 1 part by mass relative to 100 parts by mass of PVA. The same operation as in Example 3 was performed to obtain a water-soluble film. The rate of decrease of the volatile components of the film-making stock solution on the support under this condition was 2.2% by mass / second. The contact angle, swelling degree, complete dissolution time and sealing strength at 165°C of the water-soluble film were measured using the obtained water-soluble film. Furthermore, a transportation test of a package obtained by packaging a model detergent with the water-soluble film was carried out. The results are shown in Table 1.

[0185] <Comparative Example 4>

[0186] The surface temperature of the support was changed to 70°C, the temperature of the hot air blown to the entire surface not in contact with the support was changed to 80°C, and the surface temperature of the heat treatment roller was changed to 90°C. The same operation as in Example 1 was performed to obtain a water-soluble film. The rate of decrease of the volatile components of the film-making stock solution on the support under this condition was 0.4 mass% / second. The contact angle, swelling degree, complete dissolution time and sealing strength at 165°C of the water-soluble film were measured using the obtained water-soluble film. Furthermore, a transportation test of a package obtained by packaging a model lotion with the water-soluble film was carried out. The results are shown in Table 1.

[0187] <Comparative Example 5>

[0188] The draft ratio between the T die and the support was changed to 3, the surface temperature of the support was changed to 105°C, and the temperature of the hot air blown to the entire surface not in contact with the support was changed to 105°C. Except for this, the same operation as in Example 1 was performed to obtain a water-soluble film. The rate of decrease of the volatile components of the film-making stock solution on the support under this condition was 7.2 mass % / second. The contact angle, swelling degree, complete dissolution time and sealing strength at 165°C of the water-soluble film were measured using the obtained water-soluble film. Furthermore, a transportation test of a package obtained by packaging a model lotion with the water-soluble film was carried out. The results are shown in Table 1.

[0189] <Reference Example 1>

[0190] The water-soluble film obtained in Example 3 was subjected to hot air, and its 165°C seal strength was measured without immersion in the model detergent in the above-mentioned method for measuring the 165°C seal strength. The results are shown in Table 1. In the case of not immersing in the model detergent, the 165°C seal strength was higher than that of Example 3 in which the film was immersed in the model detergent.

[0191] [Table 1]

[0192] < / pva>

Claims

1. A water-soluble film comprising polyvinyl alcohol having a degree of polymerization of 100 to 3000 and 1 to 50 parts by mass of a polyol plasticizer based on 100 parts by mass of the polyvinyl alcohol, The water-soluble film was immersed in a model detergent containing 8.6 mass % of monoethanolamine, 23.8 mass % of dodecylbenzenesulfonic acid, 9.5 mass % of propylene glycol, 23.8 mass % of lauryl alcohol ethoxylate-7-ethylene oxide adduct, 19.1 mass % of oleic acid, 9.5 mass % of diethylene glycol and 5.7 mass % of water under an environment of 23° C. and 50% RH for 24 hours. When deionized water was dropped onto the surface of the film, the contact angle after 6 seconds of dropping was 22° or more and 35° or less. After the water-soluble film is immersed in the model detergent at 23°C and 50% RH for 24 hours, the complete dissolution time when immersed in deionized water at 5°C is within 100 seconds, and The swelling degree of the water-soluble film when immersed in the model detergent at 23° C. and 50% RH for 1 hour was 30 to 50%.

2. The water-soluble film according to claim 1, wherein The water-soluble film was immersed in the model detergent under an environment of 23° C. and 50% RH for 24 hours and then heat-sealed at 165° C. The seal strength was 2.0 to 10.0 N / 15 mm.

3. The water-soluble film according to claim 1, wherein The polyvinyl alcohol is a carboxylic acid-modified or sulfonic acid-modified polyvinyl alcohol having a saponification degree of 85 mol % or more. The water-soluble film according to claim 1 , which has a thickness of 5 to 80 μm.

5. A method for producing a water-soluble film, the method comprising producing the water-soluble film according to any one of claims 1 to 4, In a method for producing a water-soluble film in which a film-forming solution containing polyvinyl alcohol is cast from a mold through a die lip in a film-like state on a support and then dried, the draw ratio obtained by dividing the linear velocity of the support on which the film-forming solution is to be cast by the linear velocity of the film-forming solution in the die lip is 2 to 60, and the rate of reduction of the volatile components of the film-forming solution on the support is 0.5 to 7% by mass / second.

6. The method for producing a water-soluble film according to claim 5, wherein: The stretch ratio obtained by dividing the linear velocity of the support on which the film-forming stock solution is cast by the winding velocity of the dried film is 0.95 to 1.

8.

7. The method for producing a water-soluble film according to claim 5 or 6, comprising: A step of heat treating the water-soluble film at 80 to 300°C.

8. A packaging body, wherein The water-soluble film according to any one of claims 1 to 4 contains a drug.

9. The packaging body according to claim 8, wherein: The medicament is a pesticide, a detergent or a disinfectant.

10. The packaging body according to claim 8 or 9, wherein: The medicine is in liquid form.