Vacuum isothermal forging method of 3D printed blank of titanium alloy integral disc shaft forging

By employing vacuum isothermal forging and segmented deformation methods, the problems of residual stress and poor plasticity in 3D-printed titanium alloy integral disc shaft forgings have been solved, enabling the production of low-cost, high-quality, and long-life titanium alloy integral disc shaft forgings.

CN116372075BActive Publication Date: 2024-11-01GUIZHOU ZIRCON TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310075271.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-07
Publication Date
2024-11-01
Estimated Expiration
2043-02-07

AI Technical Summary

Technical Problem

Existing technologies are insufficient to meet the requirements of advanced aero-engines for low cost, high quality and long service life of integral titanium alloy disc shaft forgings, especially in the case of high residual stress, poor plasticity, porosity defects and uneven microstructure and properties during the 3D printing process.

Method used

The vacuum isothermal forging method is adopted. By designing hollow billets and segmented deformation, the forging is carried out in a vacuum state using isothermal forging dies. Combined with solution treatment and aging heat treatment, it is ensured that the billet is completely transformed into a uniform TC17 titanium alloy β phase region structure at high temperature.

Benefits of technology

Near-net-shape forming of integral titanium alloy disc shaft forgings has been achieved, reducing production costs, improving dimensional accuracy and microstructure, solving the problems of residual stress and poor plasticity during 3D printing, and extending the service life of forgings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116372075B_ABST
    Figure CN116372075B_ABST
Patent Text Reader

Abstract

The invention discloses a vacuum isothermal forging method of a 3D printed blank of a titanium alloy integral disc shaft forging, and the steps are: 3D printing powder titanium alloy to prepare a hollow intermediate blank; under vacuum, preheating the surface temperature of the intermediate blank and the mold to 300℃±10℃ and applying lubricant, heating the intermediate blank and the mold to 50℃ above the phase change point of the titanium alloy; positioning the intermediate blank in the mold; the disc-shaped blank of the intermediate blank is correspondingly installed in the disc-shaped cavity of the mold cavity, the transition blank of the intermediate blank is correspondingly installed in the transition cavity of the mold cavity, the journal blank of the intermediate blank is correspondingly installed in the journal cavity of the mold cavity, the upper die cone block of the upper forging die is inserted into the middle and upper part of the middle hole of the intermediate blank, and the lower die cone block of the lower forging die is inserted into the middle and lower part of the middle hole of the intermediate blank; starting the forging press to apply a pressure of 40MN~60MN to the intermediate blank through the mold to deform it into a hollow titanium alloy integral disc shaft forging at a pressing speed of 0.08mm / s in the mold cavity. The method is mainly used for the forming of integral disc shaft forgings of aircraft engines.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a forging method of a titanium alloy forging, and in particular to a vacuum isothermal forging method of a 3D printed blank of a titanium alloy integral disc shaft forging. Background Art

[0002] Aero-engine titanium alloy integral disk shaft forgings, such as TC17 three-level disk shaft and other large forgings, often require excellent organization and performance due to the harsh working environment and complex force, in order to adapt to the extremely harsh working environment such as high temperature, high stress, high speed, high-speed airflow, etc. After the titanium alloy integral disk shaft forging is processed into a part, there is an internal through hole in the center. Since the titanium alloy integral disk shaft forging is a variable cross-section shape composed of a disk body, a transition zone and a journal body, the ratio of the outer diameter of the disk body to the outer diameter of the bottom end of the journal body is as high as 3.7:1, and the cross-section change from the disk body to the journal body is large, the journal body is prone to be insufficiency during the forming process, and due to the limitations of technological development, titanium alloy integral disk shaft forgings can only be forged into solid forgings. With the replacement of aero-engines, advanced and new aero-engines such as high thrust-to-weight ratio turbofan engines have put forward higher requirements on the organization and performance, dimensional accuracy, manufacturing cost and service life of titanium alloy integral disk shaft forgings.

[0003] In order to obtain titanium alloy integral disc shaft forgings that are close to the shape of parts, people tried to directly print hollow titanium alloy integral disc shaft forgings through 3D printing. However, after testing, the organization and performance of the hollow titanium alloy integral disc shaft forgings printed by 3D printing could not meet the design and use requirements of aircraft engines. The main reasons are as follows: ① Since 3D printing is point-by-point and layer-by-layer solidification, corresponding shear or tensile forces will be formed between adjacent points due to thermal effects, resulting in large residual stress inside the printed titanium alloy integral disc shaft forgings. Even after long-term annealing, the residual stress level is still higher than that of traditional forgings; ② 3D printing is prone to incomplete fusion of powders and defects such as pores due to insufficient or excessive energy, causing fatigue fracture of parts; ③ 3D printing is composed of countless points melting and solidification, with large residual stress, and sufficient, continuous and effective slip cannot be formed on a macro scale, resulting in poor plasticity of 3D printed parts.

[0004] The Chinese invention patent specification CN101758159A published on June 30, 2010 discloses a near-isothermal forging method for a titanium alloy integral disc shaft forging. The billet making steps of the method are as follows: titanium alloy bar → blanking → primary bar ingot → heating → upsetting → primary round cake → heating → drawing + forging → primary square billet → heating → upsetting + rolling → secondary round cake → heating → drawing + forging → secondary square billet → heating → upsetting + rolling → tertiary round cake → heating → drawing + forging → tertiary square billet → rolling → round billet → processing → conical billet → heating → die forging → primary pre-forging billet → processing → secondary pre-forging billet; the forging steps of the method are as follows: heating the forging die to 25°C below the phase transition point of the titanium alloy, applying lubricant on the surface of the die cavity, preheating the secondary pre-forging billet The material is prepared, and glass lubricant is evenly sprayed on its surface. The blank is then heated to 35°C above the phase change point and then loaded into the die sleeve and the lower forging die. The lower positioning hole of the secondary pre-forging blank cooperates with the lower die convex block of the lower forging die and is positioned by the lower die convex block. The forging press is started to close the upper forging die, the die sleeve and the lower forging die. The upper positioning hole of the secondary pre-forging blank cooperates with the upper die convex block of the upper forging die and is positioned by the upper die convex block. The forging press is used to make the forging die apply a pressure of 40MN to 60MN to the secondary pre-forging blank so that the blank is deformed by 25% at a pressing speed of 0.08mm / s in the die cavity and then forged into an integral disc shaft forging.

[0005] The method produces a pre-forged billet through seven fires, during which the primary ingot is continuously subjected to upsetting, elongating and forging a square billet, upsetting and rolling, elongating and forging a square billet, etc., and then the square billet is rolled to obtain a round billet, and then the round billet is processed into a conical billet, and then the conical billet is forged by a die to obtain a pre-forged billet, and then the pre-forged billet is processed into a secondary pre-forged billet with positioning holes on the upper and lower end faces, and finally the secondary pre-forged billet is forged into a titanium alloy integral disc shaft forging. Moreover, for forging TC17 titanium alloy integral disc shaft forgings, the alloy is a near-β-type titanium alloy, and the billet is made of large-sized ingot smelting and rolled bars. Large-sized ingots are prone to segregation, β spots and other defects during smelting, and multiple fires of forging are prone to cause local heating to form large grains, which affects the structure and performance of the forgings.

[0006] It can be seen that the blank making process of this method is very cumbersome and complicated. It not only requires the investment of heating equipment, forging equipment, machining equipment and other devices, but also is time-consuming, labor-intensive, consumes a lot of materials, wastes resources and energy, greatly increases production costs, and is not conducive to market competition. The blanks made by this method are solid blanks with blind holes, and the forged forgings are solid integral disc shaft forgings with blind holes. It is impossible to achieve near-net forming along the distribution of the forgings along the shape of the parts, and it is impossible to obtain forgings with high dimensional accuracy; and because the central part of the solid integral disc shaft forging is thick and large, it is not easy to forge through during forging, which affects its organization and performance. In addition, the central part of the integral disc shaft forging is the main stress-bearing part during use, which will affect its service life. This method uses a combined die, which is more complicated to process and assemble. The forged forgings are prone to form indentations and burrs at the gaps of the die combination, which affects the material flow of the blank when it is formed in the die, thereby affecting the dimensional accuracy and increasing the grinding workload. This method uses near-isothermal forging with a die temperature close to the billet temperature, and is carried out under atmospheric conditions. During the forging process, the die temperature drops rapidly, which easily produces a cold die effect. All of the above factors make it impossible for the forging to achieve superplastic forming and obtain better structure and performance.

[0007] In summary, the forging method cannot meet the high requirements of advanced and new aircraft engines for low cost, high quality and long life of titanium alloy integral disc shaft forgings. Summary of the invention

[0008] The technical problem to be solved by the present invention is to provide a vacuum isothermal forging method for a hollow billet to realize the 3D printing of a titanium alloy integral disc shaft forging. The method obtains a titanium alloy integral disc shaft forging with high dimensional accuracy and organizational properties through reasonable billet and forging size design and segmented deformation.

[0009] In order to solve the above technical problems, the vacuum isothermal forging method of the titanium alloy integral disc shaft forging 3D printing blank of the present invention comprises the following steps:

[0010] A powder titanium alloy with a particle size of 60-200 meshes made of a small-sized ingot is made into an intermediate blank by 3D printing, and then subjected to stress relief annealing. The intermediate blank is a hollow blank similar to a funnel shape, which is smoothly connected into one by an upper disc blank and a lower journal blank through a transition blank. There is a through middle hole in the intermediate blank along the axial center from the upper end face of the disc blank to the bottom end face of the journal blank;

[0011] An isothermal forging die is provided, the isothermal forging die comprising an upper forging die and a lower forging die; the upper forging die is an integral die, and has an upper die cone block at the center of the bottom surface of the upper forging die for cooperating with the middle hole of the intermediate blank and forming an upper cone hole of a titanium alloy integral disc shaft forging; the lower forging die is also an integral die, and has a lower die cone block at the center of the bottom surface of the lower forging die cavity for cooperating with the middle hole of the intermediate blank and forming a lower cone hole of the titanium alloy integral disc shaft forging; the upper forging die and the lower forging die are combined to form a die cavity of the titanium alloy integral disc shaft forging, the upper part of the die cavity is a disc-shaped cavity, the middle part is a transition cavity, and the lower part is a journal cavity;

[0012] Under vacuum, first preheat the intermediate blank and the opened mold to a surface temperature of 300°C ± 10°C, and evenly spray lubricant on the surface of the intermediate blank and the mold cavity; then heat the intermediate blank and the mold to 50°C above the phase transition point of the titanium alloy, and load the intermediate blank into the mold cavity, so that the disc-shaped blank of the intermediate blank is installed in the disc-shaped cavity position of the mold cavity, the transition blank of the intermediate blank is installed in the transition cavity position of the mold cavity, and the journal blank of the intermediate blank is installed in the journal cavity position of the mold cavity. The upper die cone block of the upper forging die is inserted into the middle and upper part of the middle hole of the intermediate blank, and the lower die cone block of the lower forging die is inserted into the middle and lower part of the middle hole of the intermediate blank, so that the intermediate blank is firmly positioned in the mold cavity;

[0013] Under vacuum, start the forging press to close the upper forging die and the lower forging die. The forging press applies a pressure of 40MN to 60MN to the intermediate blank through the die, so that the intermediate blank is deformed in sections at a pressing speed of 0.08mm / s in the die cavity to become a hollow titanium alloy integral disc shaft forging. The sectioned deformation of the intermediate blank during the forging forming process in the die cavity is as follows: the deformation amount of the disc-shaped blank of the intermediate blank in the disc-shaped cavity of the die cavity is 60%, the deformation amount of the transition blank of the intermediate blank in the transition cavity of the die cavity is 50%, and the deformation amount of the journal blank of the intermediate blank in the journal cavity of the die cavity is 30%.

[0014] The upper part of the titanium alloy integral disc-shaft forging forged by the above method is a disc-shaped body, and the lower part is a journal body, and the connecting portion between the disc-shaped body and the journal body is a transition zone; the titanium alloy integral disc-shaft forging has an upper tapered hole along the axial center from the upper end face of the disc-shaped body to a position slightly below the lower part of the transition zone, and connected to the upper tapered hole is a lower tapered hole located in the axial center of the journal body and extending to the bottom end face of the journal body. The upper tapered hole and the lower tapered hole pass through from the upper end face to the lower end face of the titanium alloy integral disc-shaft forging to form the inner hole of the titanium alloy integral disc-shaft forging.

[0015] The dimensional relationship between the intermediate blank and the titanium alloy integral disc shaft forging is as follows:

[0016] ①h1÷H1=K×D1÷d1; where:

[0017] h1 is the height of the disc-shaped blank on the upper part of the intermediate blank;

[0018] H1 is the height of the upper disc-shaped body of the titanium alloy integral disc shaft forging;

[0019] K is the radial and axial forming speed multiplier of the intermediate blank, and K=2.3;

[0020] D1 is the outer diameter of the upper disc-shaped body of the titanium alloy integral disc shaft forging;

[0021] d1 is the outer diameter of the upper disc blank of the intermediate blank.

[0022] ②α1=α2;h2=H2;where:

[0023] α1 is the inclination angle of the transition blank in the middle of the intermediate blank;

[0024] α2 is the inclination angle of the transition zone in the middle of the titanium alloy integral disc shaft forging;

[0025] h2 is the height of the transition billet in the middle of the intermediate billet;

[0026] H2 is the height of the transition zone in the middle of the titanium alloy integral disc shaft forging.

[0027] ③0.5H≤h3≤0.8H, b1=0.4B1; where:

[0028] H is the height of the titanium alloy integral disc shaft forging;

[0029] h3 is the height of the journal blank at the lower part of the intermediate blank;

[0030] b1 is the average wall thickness of the lower journal blank of the intermediate blank;

[0031] B1 is the average wall thickness of the lower journal body of the titanium alloy integral disc shaft forging.

[0032] ④D5=(D2+D4)÷K÷2;(d2+d4+d5+d6)÷4=1.06×K×D5;Where:

[0033] D5 is the inner diameter of the intersection of the upper tapered hole and the lower tapered hole in the titanium alloy integral disc shaft forging;

[0034] D2 is the inner diameter of the top of the upper disc-shaped body of the titanium alloy integral disc shaft forging;

[0035] D4 is the inner diameter of the bottom end of the lower journal body of the titanium alloy integral disc shaft forging;

[0036] K is the radial and axial forming speed multiplier of the intermediate blank, and K=2.3;

[0037] d2 is the inner diameter of the top of the disc-shaped blank on the intermediate blank;

[0038] d4 is the inner diameter of the bottom end of the lower journal blank of the intermediate blank;

[0039] d5 is the inner diameter of the conical turning point of the inner hole of the transition blank in the middle of the intermediate blank;

[0040] d6 is the inner diameter of the junction between the inner hole of the lower journal blank of the intermediate blank and the inner hole of the transition blank;

[0041] 1.06 is the inner hole forming safety factor of the titanium alloy integral disc shaft forging.

[0042] For the isothermal forging die provided above, an upper die push rod that can move up and down for ejecting the titanium alloy integral disc shaft forging is arranged in the upper forging die of the die at a certain distance from the upper outer edge of the die cavity, and the number of the upper die push rods is four and evenly distributed in the upper forging die and passes through the upper end surface of the upper forging die; a lower die push rod that can move up and down for ejecting the titanium alloy integral disc shaft forging is arranged at the root of the lower die cone block of the lower forging die, located at the bottom end of the die cavity, and the number of the lower die push rods is four and evenly distributed in the lower forging die and passes through the bottom end surface of the lower forging die.

[0043] The stress relief annealing is performed by heating the intermediate billet to 600°C, keeping the temperature for 12 hours, and air cooling.

[0044] The material grade of the above-mentioned powdered titanium alloy is TC17.

[0045] The above-mentioned titanium alloy integral disc shaft forging is subjected to solution treatment + aging heat treatment after forging. The solution treatment is to heat the titanium alloy integral disc shaft forging to 800℃±10℃, keep it warm for 4 hours, and then put it into water for rapid cooling, i.e., water quenching. The aging heat treatment is to heat the titanium alloy integral disc shaft forging after the solution treatment to 630℃±10℃, keep it warm for 8 hours, and then air cool it.

[0046] Compared with the prior art, the present invention has the following beneficial effects:

[0047] The vacuum isothermal forging method of the 3D printed blank of the titanium alloy integral disc-shaft forging described in the present invention eliminates the cold die effect and realizes superplastic forming by designing the intermediate blank into a hollow blank having a disc-shaped blank, a transition blank and a journal blank and performing 3D printing, and then deforming them into the disc-shaped body, transition body and journal body of the titanium alloy integral disc-shaft forging in the disc-shaped cavity, transition cavity and journal cavity of the isothermal forging die accordingly. Isothermal forging is performed under vacuum conditions, thereby eliminating the cold die effect and realizing superplastic forming. Compared with the prior art which uses large-sized ingots for smelting and rolling rods to make billets, the present invention uses small-sized ingots to produce powdered titanium alloy, which greatly reduces the risk of forming β-spot defects, and the billet does not have enough time and thermodynamic conditions to form segregation during the 3D printing process, and will not produce defects such as segregation and β-spots, nor does it require multiple forgings to make billets, which will cause large grains to affect the microstructure and properties of the forgings; compared with the prior art which has problems such as cumbersome and complex billet making process, high equipment investment, long processing cycle, large material consumption, large waste of resources and energy, high production cost, and weak market competitiveness, the billet making process of this method is relatively simple, with low equipment investment, short production cycle, low material consumption, resource and energy saving, low manufacturing cost, and strong market competitiveness. The hollow titanium alloy integral disc shaft forgings produced can be distributed along the shape of the parts, and the central stress-bearing part of the titanium alloy integral disc shaft forging can be forged through, thereby realizing the near-net forming of the hollow titanium alloy integral disc shaft forgings, and obtaining titanium alloy integral disc shaft forgings with high dimensional accuracy, microstructure and properties, and service life.

[0048] The present invention obtains the shape and size of the optimal intermediate blank and the titanium alloy integral disc shaft forging suitable for 3D printing and forging of the present invention, as well as the shape and size of the optimal titanium alloy integral disc shaft forging, by creatively designing the shape and size of the intermediate blank and the titanium alloy integral disc shaft forging, and the shape and size of the optimal titanium alloy integral disc shaft forging. When such an intermediate blank is used to forge such a titanium alloy integral disc shaft forging, segmented deformation can be smoothly achieved, so that the disc-shaped blank of the intermediate blank is deformed by 60% in the disc-shaped cavity of the mold cavity to become the disc-shaped body of the titanium alloy integral disc shaft forging, the transition blank of the intermediate blank is deformed by 50% in the transition cavity of the mold cavity to become the transition zone of the titanium alloy integral disc shaft forging, and the journal blank of the intermediate blank is deformed by 30% in the journal cavity of the mold cavity to become the journal body of the titanium alloy integral disc shaft forging; such segmented deformation method can ensure that the large head part of the blank is greatly deformed, and the small head part is slightly deformed, which overcomes the problems of large cross-sectional changes and insufficient filling of the journal body during the forming process of the hollow titanium alloy integral disc shaft forging, and The same deformation in different parts leads to uneven organizational properties; and such forming method is adopted and both the intermediate billet and the mold are heated to 50°C above the phase transformation point of the titanium alloy for isothermal forging. Compared with the prior art that adopts the traditional method of smelting and rolling the billet made of bars and heats it to 35°C above the phase transformation point for forging, the 3D printed billet close to the fine-grained cast structure can be completely transformed into a more uniform and fine-grained structure in the β phase region of the TC17 titanium alloy at a higher temperature, which can release the residual stress generated by the 3D printed billet, and the defects of the compacted powder titanium alloy 3D printing such as incomplete fusion and pores can be overcome by superplastic isothermal forging under vacuum conditions. The problem of poor plasticity of the 3D printed billet can also be overcome.

[0049] The upper forging die and the lower forging die of the method both adopt an integral structure. Compared with the combined die in the prior art, the processing and assembly thereof are relatively simple, and can avoid the indentations and burrs on the forging surface caused by the joint position of the combined die, so that the material flow is smoother when the blank is formed in the die, which is beneficial to improving the surface quality of the forging and improving the dimensional accuracy, and reducing the amount of grinding.

[0050] In summary, the forging method described in the present invention can meet the high requirements of advanced and new aircraft engines for low cost, high quality and long life of titanium alloy integral disc shaft forgings. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0052] Figure 1 This is the structure diagram of the intermediate billet made by 3D printing powder titanium alloy.

[0053] Figure 2 It is a structural diagram of the titanium alloy integral disc shaft forging described in the present invention.

[0054] Figure 3 It is a structural diagram of the die used for the vacuum isothermal forging of the present invention.

[0055] Figure 4 yes Figure 1 The intermediate billet shown is loaded into Figure 3 Assembly drawing of the mold shown.

[0056] Figure 5 yes Figure 1 The intermediate billet shown is Figure 3 The die forging shown is Figure 2 The state diagram of the titanium alloy integral disc shaft forging is shown. DETAILED DESCRIPTION

[0057] To implement the vacuum isothermal forging method of the titanium alloy integral disc shaft forging 3D printed blank described in the present invention, it is necessary to provide relevant equipment and facilities such as a 3D printer, a forging press, a heating device, a manipulator and a vacuum forging chamber.

[0058] The process steps of the present invention are described in detail below using TC17 powder titanium alloy as an example:

[0059] Step 1: Determine the shape and size of the billet and forging.

[0060] like Figure 1 As shown, the blank required for the titanium alloy integral disc shaft forging of the present invention is an intermediate blank 10, which is similar to a funnel shape, and is smoothly connected into one by an upper disc blank 11 and a lower journal blank 13 through a transition blank 12. There is a through middle hole 10a along the axial center of the intermediate blank 10 from the upper end surface of the disc blank 11 to the bottom end surface of the journal blank 13, that is, the intermediate blank 10 is a hollow blank. The relevant dimensions of the intermediate blank 10 are as follows:

[0061] d1 is the outer diameter of the upper disc-shaped blank 11 of the intermediate blank 10;

[0062] d2 is the inner diameter of the top of the disc-shaped blank 11 on the upper part of the intermediate blank 10;

[0063] d3 is the outer diameter of the bottom end of the journal blank 13 at the lower part of the intermediate blank 10;

[0064] d4 is the inner diameter of the bottom end of the journal blank 13 at the lower part of the intermediate blank 10;

[0065] d5 is the inner diameter of the conical turning point of the inner hole of the transition blank 12 in the middle of the intermediate blank 10;

[0066] d6 is the inner diameter of the junction between the inner hole of the journal blank 13 at the lower part of the intermediate blank 10 and the inner hole of the transition blank 12;

[0067] Among them: d2>d5>d6>d4.

[0068] h1 is the height of the disc-shaped blank 11 on the upper portion of the intermediate blank 10;

[0069] h2 is the height of the transition blank 12 in the middle of the intermediate blank 10;

[0070] α1 is the inclination angle of the transition blank 12 in the middle of the intermediate blank 10;

[0071] h3 is the height of the journal blank 13 at the lower part of the intermediate blank 10;

[0072] h is the height of the intermediate billet 10, and: h=h1+h2+h3.

[0073] like Figure 2 As shown, the titanium alloy integral disc shaft forging 20 of the present invention has a disc-shaped body 21 at the upper part and a journal body 23 at the lower part. The connecting part between the disc-shaped body 21 and the journal body 23 is a transition zone 22. The titanium alloy integral disc shaft forging 20 has an upper tapered hole 21a from the upper end face of the disc-shaped body 21 to a position slightly below the lower part of the transition zone 22 along the axial center. The upper tapered hole 21a is connected to the lower tapered hole 23a located in the axial center of the journal body 23 and extending to the bottom end face of the journal body 23. The upper tapered hole 21a and the lower tapered hole 23a penetrate from the upper end face of the titanium alloy integral disc shaft forging 20 to the lower end face to form the inner hole of the titanium alloy integral disc shaft forging 20, that is, the titanium alloy integral disc shaft forging 20 is a hollow forging. The relevant dimensions of the titanium alloy integral disc shaft forging 20 are as follows:

[0074] D1 is the outer diameter of the upper disc-shaped body 21 of the titanium alloy integral disc-shaft forging 20;

[0075] D2 is the inner diameter of the top of the upper disc-shaped body 21 of the titanium alloy integral disc-shaft forging 20;

[0076] D3 is the outer diameter of the bottom end of the lower journal body 23 of the titanium alloy integral disc shaft forging 20;

[0077] D4 is the inner diameter of the bottom end of the lower journal body 23 of the titanium alloy integral disc shaft forging 20;

[0078] D5 is the inner diameter of the intersection of the upper tapered hole 21a and the lower tapered hole 23a in the titanium alloy integral disc shaft forging 20;

[0079] H1 is the height of the upper disc-shaped body 21 of the titanium alloy integral disc-shaft forging 20;

[0080] H2 is the height of the transition zone 22 in the middle of the titanium alloy integral disc shaft forging 20;

[0081] α2 is the inclination angle of the transition zone 22 in the middle of the titanium alloy integral disc shaft forging 20;

[0082] H3 is the height of the lower journal body 23 of the titanium alloy integral disc shaft forging 20;

[0083] H is the height of the titanium alloy integral disc-shaft forging 20 , and: H=H1+H2+H3.

[0084] Figure 1 The dimensions of the intermediate blank 10 shown and Figure 2 The relationship between the dimensions of the titanium alloy integral disc shaft forging 20 shown is as follows:

[0085] ① h1÷H1=K×D1÷d1;

[0086] Wherein: K is the radial and axial forming speed multiplier coefficient of the intermediate blank 10, and the present invention takes K=2.3.

[0087] The purpose of such a design is to limit the outer diameter d1 and height h1 of the intermediate blank 10 and the disc-shaped blank 11, so that the disc-shaped blank 11 can be formed synchronously with the journal blank 13, thereby preventing the disc-shaped blank 11 from being filled with the disc-shaped body 21 of the titanium alloy integral disc-shaft forging 20 too early during the forging process to form burrs, thereby affecting the dimensional accuracy of the forging.

[0088] ② α1=α2;h2=H2;

[0089] The purpose of this design is to make the outer edge of the transition blank 12 in the middle of the intermediate blank 10 coincide with the outer edge of the transition zone 22 in the middle of the titanium alloy integral disc-shaft forging 20. During the forging process, the blank of the transition blank 12 can flow in a balanced manner toward the disc-shaped body 21, the journal body 23 and the inner hole of the titanium alloy integral disc-shaft forging 20, ensuring that the filling process is carried out evenly, which is conducive to obtaining a forging with uniform structure.

[0090] ③ 0.5H≤h3≤0.8H, b1=0.4B1;

[0091] Wherein: b1 is the average wall thickness of the lower journal blank 13 of the intermediate blank 10; B1 is the average wall thickness of the lower journal body 23 of the titanium alloy integral disc shaft forging 20;

[0092] The purpose of such a design is to enable the journal blank 13 at the lower part of the intermediate blank 10 to obtain sufficient deformation when deforming into the journal body 23 at the lower part of the titanium alloy integral disc shaft forging 20, so as to avoid folding or extrusion filling.

[0093] ④ D5=(D2+D4)÷K÷2; (d2+d4+d5+d6)÷4=1.06×K×D5;

[0094] Wherein: K is the radial and axial forming speed multiplier coefficient of the intermediate blank 10 , and the present invention takes K=2.3; 1.06 is the inner hole forming safety factor of the titanium alloy integral disc-shaft forging 20 .

[0095] The purpose of this design is to ensure that the intersection of the upper tapered hole 21a and the lower tapered hole 23a of the titanium alloy integral disc-shaft forging 20 can be filled synchronously or finally with the outer edge of the disc-shaped body 21 and the bottom of the journal body 23 during forging, avoiding premature filling and forming burrs.

[0096] Step 2: Determine the shape and size of the forging die.

[0097] like Figure 3 As shown, the isothermal forging die 30 used to implement the present invention includes an upper forging die 31 and a lower forging die 32. The upper forging die 31 is an integral die, and the center of the bottom surface of the upper forging die 31 has an upper die cone block 31a for cooperating with the middle hole 10a of the intermediate blank 10 and forming the upper cone hole 21a of the titanium alloy integral disc shaft forging 20; the lower forging die 32 is also an integral die, and the center of the bottom surface of the cavity of the lower forging die 32 has a lower die cone block 32a for cooperating with the middle hole 10a of the intermediate blank 10 and forming the lower cone hole 23a of the titanium alloy integral disc shaft forging 20. The upper forging die 31 and the lower forging die 32 are combined to form the die cavity 30a of the titanium alloy integral disc shaft forging 20. To facilitate the removal of forgings, an upper die push rod 31b that can move up and down for ejecting the titanium alloy integral disc shaft forging 20 is arranged at a certain distance from the upper outer edge of the mold cavity 30a in the upper forging die 31, and the upper die push rods 31b are four and evenly distributed in the upper forging die 31 and pass through the upper end surface of the upper forging die 31; a lower die push rod 32b that can move up and down for ejecting the titanium alloy integral disc shaft forging 20 is arranged at the root of the lower die cone block 32a of the lower forging die 32, located at the bottom end of the mold cavity 30a, and the lower die push rods 32b are four and evenly distributed in the lower forging die 32 and pass through the bottom end surface of the lower forging die 32. The upper part of the mold cavity 30a is a disc-shaped cavity 30a1, the middle part is a transition cavity 30a2, and the lower part is a journal cavity 30a3. The disc-shaped cavity 30a1 corresponds to the disc-shaped body 21 of the titanium alloy integral disc-shaft forging 20 and has the same size and shape. The transition cavity 30a2 corresponds to the transition zone 22 of the titanium alloy integral disc-shaft forging 20 and has the same size and shape. The journal cavity 30a3 corresponds to the journal body 23 of the titanium alloy integral disc-shaft forging 20 and has the same size and shape. In other words, the shape and size of the mold cavity 30a are exactly the same as the shape and size of the titanium alloy integral disc-shaft forging 20.

[0098] Step 3: 3D printing.

[0099] The TC17 powder titanium alloy with a particle size of 60-200 mesh made from small-sized ingots was 3D printed into Figure 1 The intermediate blank 10 shown in the figure is subjected to stress relief annealing after being manufactured. The stress relief annealing is performed by heating the intermediate blank 10 to 600° C., keeping the temperature for 12 hours, and air cooling.

[0100] Step 4: Assemble the mold.

[0101] like Figure 4 As shown, in a vacuum state, for example, in a sealed vacuum forging chamber (not shown in the drawings, the forging chamber is equipped with a forging press, a heating furnace, an automatic lubricant spraying device, and an automatic control manipulator for clamping, transferring and loading and unloading the blank, etc.), first preheat the intermediate blank 10 and the opened mold 30 to a surface temperature of 300°C ± 10°C, and evenly spray a lubricant, such as a glass lubricant, on the surface of the intermediate blank 10 and the mold cavity 30a; then heat the intermediate blank 10 and the mold 30 to 50°C above the phase transition point of the TC17 titanium alloy, and load the intermediate blank 10 into the mold cavity 30a. a, so that the disc-shaped blank 11 of the intermediate blank 10 is installed in the position of the disc-shaped cavity 30a1 of the mold cavity 30a, the transition blank 12 of the intermediate blank 10 is installed in the position of the transition cavity 30a2 of the mold cavity 30a, the journal blank 13 of the intermediate blank 10 is installed in the position of the journal cavity 30a3 of the mold cavity 30a, the upper die cone block 31a of the upper forging die 31 is inserted into the middle and upper part of the middle hole 10a of the intermediate blank 10, and the lower die cone block 32a of the lower forging die 32 is inserted into the middle and lower part of the middle hole 10a of the intermediate blank 10, so that the intermediate blank 10 is firmly positioned in the mold cavity 30a to complete the molding process.

[0102] Step 5: Vacuum isothermal forging.

[0103] like Figure 5 As shown, in a vacuum state, the forging press is started to close the upper forging die 31 and the lower forging die 32, and the forging press applies a pressure of 40MN to 60MN to the intermediate blank 10 through the die 30, so that the intermediate blank 10 is deformed in the die cavity 30a at a pressing speed of 0.08mm / s into the following Figure 2 The titanium alloy integral disc shaft forging 20 shown in the figure; the segmented deformation of the intermediate blank 10 in the die cavity 30a during the forging process is as follows: the deformation of the disc-shaped blank 11 of the intermediate blank 10 in the disc-shaped cavity 30a1 of the die cavity 30a is 60%, the deformation of the transition blank 12 of the intermediate blank 10 in the transition cavity 30a2 of the die cavity 30a is 50%, and the deformation of the journal blank 13 of the intermediate blank 10 in the journal cavity 30a3 of the die cavity 30a is 30%. After forging, the titanium alloy integral disc shaft forging 20 is pushed out of the upper forging die 31 by the upper die push rod 31b, and the titanium alloy integral disc shaft forging 20 is pushed out of the lower forging die 32 by the lower die push rod 32b, and then the titanium alloy integral disc shaft forging 20 is taken out of the die 30, and the whole forging process is completed.

[0104] In the forging process, the initial forging temperature is 50°C above the phase transition point of the TC17 titanium alloy, and the final forging temperature is ≥750°C; when the TC17 titanium alloy material is used for forging, it is tested that its phase transition point is 895°C.

[0105] Step 6: Heat treatment after forging

[0106] After forging, the titanium alloy integral disc shaft forging 20 is subjected to heat treatment, i.e., solid solution treatment + aging treatment. The solid solution treatment is to heat the titanium alloy integral disc shaft forging 20 to 800°C ± 10°C, keep it warm for 4 hours, and then put it into water for rapid cooling (water quenching); the aging treatment is to heat the titanium alloy integral disc shaft forging 20 after solid solution treatment to 630 ± 10°C, keep it warm for 8 hours, and then air cool it.

Claims

1. A vacuum isothermal forging method for 3D printing blanks of titanium alloy integral disc shaft forgings, characterized in that: The following steps are involved: A powder titanium alloy with a particle size of 60-200 meshes made of a small-sized ingot is made into an intermediate blank by 3D printing, and then subjected to stress relief annealing. The intermediate blank is a hollow blank similar to a funnel shape, which is smoothly connected into one by an upper disc blank and a lower journal blank through a transition blank. There is a through middle hole in the intermediate blank along the axial center from the upper end face of the disc blank to the bottom end face of the journal blank; An isothermal forging die is provided, the isothermal forging die comprising an upper forging die and a lower forging die; the upper forging die is an integral die, and has an upper die cone block at the center of the bottom surface of the upper forging die for cooperating with the middle hole of the intermediate blank and forming an upper cone hole of a titanium alloy integral disc shaft forging; the lower forging die is also an integral die, and has a lower die cone block at the center of the bottom surface of the lower forging die cavity for cooperating with the middle hole of the intermediate blank and forming a lower cone hole of the titanium alloy integral disc shaft forging; the upper forging die and the lower forging die are combined to form a die cavity of the titanium alloy integral disc shaft forging, the upper part of the die cavity is a disc-shaped cavity, the middle part is a transition cavity, and the lower part is a journal cavity; Under vacuum, first preheat the intermediate blank and the opened mold to a surface temperature of 300°C ± 10°C, and evenly spray lubricant on the surface of the intermediate blank and the mold cavity; then heat the intermediate blank and the mold to 50°C above the phase transition point of the titanium alloy, and load the intermediate blank into the mold cavity, so that the disc-shaped blank of the intermediate blank is installed in the disc-shaped cavity position of the mold cavity, the transition blank of the intermediate blank is installed in the transition cavity position of the mold cavity, and the journal blank of the intermediate blank is installed in the journal cavity position of the mold cavity. The upper die cone block of the upper forging die is inserted into the middle and upper part of the middle hole of the intermediate blank, and the lower die cone block of the lower forging die is inserted into the middle and lower part of the middle hole of the intermediate blank, so that the intermediate blank is firmly positioned in the mold cavity; Under vacuum, start the forging press to close the upper forging die and the lower forging die. The forging press applies a pressure of 40MN to 60MN to the intermediate blank through the die, so that the intermediate blank is deformed in sections at a pressing speed of 0.08mm / s in the die cavity to become a hollow titanium alloy integral disc shaft forging. The sectioned deformation of the intermediate blank during the forging forming process in the die cavity is as follows: the deformation amount of the disc-shaped blank of the intermediate blank in the disc-shaped cavity of the die cavity is 60%, the deformation amount of the transition blank of the intermediate blank in the transition cavity of the die cavity is 50%, and the deformation amount of the journal blank of the intermediate blank in the journal cavity of the die cavity is 30%.

2. The vacuum isothermal forging method of the titanium alloy integral disc shaft forging 3D printing blank according to claim 1, characterized in that: The upper part of the titanium alloy integral disc-shaft forging is a disc-shaped body, and the lower part is a journal body, and the connecting portion between the disc-shaped body and the journal body is a transition zone; an upper tapered hole is provided in the titanium alloy integral disc-shaft forging along the axial center from the upper end surface of the disc-shaped body to a position slightly below the lower part of the transition zone, and the upper tapered hole is connected to the lower tapered hole, which is located in the axial center of the journal body and extends to the bottom end surface of the journal body. The upper tapered hole and the lower tapered hole pass through from the upper end surface to the lower end surface of the titanium alloy integral disc-shaft forging to form the inner hole of the titanium alloy integral disc-shaft forging.

3. The vacuum isothermal forging method of the titanium alloy integral disc shaft forging 3D printing blank as claimed in claim 1 or 2, characterized in that: The dimensional relationship between the intermediate blank and the titanium alloy integral disc shaft forging is as follows: ①h1÷H1=K×D1÷d1; where: h1 is the height of the disc-shaped blank on the upper part of the intermediate blank; H1 is the height of the upper disc-shaped body of the titanium alloy integral disc shaft forging; K is the radial and axial forming speed multiplier of the intermediate blank, and K=2.3; D1 is the outer diameter of the upper disc-shaped body of the titanium alloy integral disc shaft forging; d1 is the outer diameter of the disc-shaped blank on the upper part of the intermediate blank; ②α1=α2;h2=H2;where: α1 is the inclination angle of the transition blank in the middle of the intermediate blank; α2 is the inclination angle of the transition zone in the middle of the titanium alloy integral disc shaft forging; h2 is the height of the transition billet in the middle of the intermediate billet; H2 is the height of the transition zone in the middle of the titanium alloy integral disc shaft forging; ③0.5H≤h3≤0.8H, b1=0.4B1; Where: H is the height of the titanium alloy integral disc shaft forging; h3 is the height of the journal blank at the lower part of the intermediate blank; b1 is the average wall thickness of the lower journal blank of the intermediate blank; B1 is the average wall thickness of the lower journal body of the titanium alloy integral disc shaft forging; ④D5=(D2+D4)÷K÷2;(d2+d4+d5+d6)÷4=1.06×K×D5;Where: D5 is the inner diameter of the intersection of the upper tapered hole and the lower tapered hole in the titanium alloy integral disc shaft forging; D2 is the inner diameter of the top of the upper disc-shaped body of the titanium alloy integral disc shaft forging; D4 is the inner diameter of the bottom end of the lower journal body of the titanium alloy integral disc shaft forging; K is the radial and axial forming speed multiplier of the intermediate blank, and K=2.3; d2 is the inner diameter of the top of the disc-shaped blank on the intermediate blank; d4 is the inner diameter of the bottom end of the lower journal blank of the intermediate blank; d5 is the inner diameter of the conical turning point of the inner hole of the transition blank in the middle of the intermediate blank; d6 is the inner diameter of the junction between the inner hole of the lower journal blank of the intermediate blank and the inner hole of the transition blank; 1.06 is the inner hole forming safety factor of the titanium alloy integral disc shaft forging.

4. The vacuum isothermal forging method of the titanium alloy integral disc shaft forging 3D printing blank according to claim 1, characterized in that: An upper die push rod that can move up and down and is used to eject the titanium alloy integral disc shaft forging is arranged at a certain distance from the upper outer edge of the die cavity in the upper forging die of the isothermal forging die, and the number of the upper die push rods is four and is evenly distributed in the upper forging die and passes through the upper end surface of the upper forging die; a lower die push rod that can move up and down and is used to eject the titanium alloy integral disc shaft forging is arranged at the root of the lower die cone block of the lower forging die and is located at the bottom end of the die cavity, and the number of the lower die push rods that can move up and down and is used to eject the titanium alloy integral disc shaft forging is four and is evenly distributed in the lower forging die and passes through the bottom end surface of the lower forging die.

5. The vacuum isothermal forging method of the titanium alloy integral disc shaft forging 3D printing blank according to claim 1, characterized in that: The stress relief annealing is to heat the intermediate billet to 600° C., keep the temperature for 12 hours, and then air cool.

6. The vacuum isothermal forging method of a titanium alloy integral disc shaft forging 3D printing blank as claimed in any one of claims 1, 2, 4 and 5, characterized in that: The material grade of the powdered titanium alloy is TC17.

7. The vacuum isothermal forging method of a titanium alloy integral disc shaft forging 3D printing blank as claimed in any one of claims 1, 2, 4 and 5, characterized in that: The titanium alloy integral disc shaft forging is subjected to a solid solution + aging heat treatment after forging.

8. The vacuum isothermal forging method of the titanium alloy integral disc shaft forging 3D printing blank as claimed in claim 7, characterized in that: The solution treatment is to heat the titanium alloy integral disc shaft forging to 800°C±10°C, keep it warm for 4 hours and then put it into water for rapid cooling, i.e., water quenching. The aging heat treatment is to heat the titanium alloy integral disc shaft forging after the solution treatment to 630°C±10°C, keep it warm for 8 hours and then air cool it.

9. The vacuum isothermal forging method of the titanium alloy integral disc shaft forging 3D printing blank as claimed in claim 3, characterized in that: The material grade of the powdered titanium alloy is TC17.

10. The vacuum isothermal forging method of the titanium alloy integral disk-shaft forging 3D printing blank according to claim 3, characterized in that: The titanium alloy integral disc shaft forging is subjected to a solid solution + aging heat treatment after forging.

11. The vacuum isothermal forging method of the titanium alloy integral disk-shaft forging 3D printing blank according to claim 10, characterized in that: The solution treatment is to heat the titanium alloy integral disc shaft forging to 800°C±10°C, keep it warm for 4 hours and then put it into water for rapid cooling, i.e., water quenching. The aging heat treatment is to heat the titanium alloy integral disc shaft forging after the solution treatment to 630°C±10°C, keep it warm for 8 hours and then air cool it.