A preparation method and application of NH4V3O8 based on automatic pH adjustment
The preparation process of NH4V3O8 is simplified by the method of automatic pH adjustment, and the problems of high cost and cumbersome steps in the existing technology are solved, and the preparation of NH4V3O8 with low energy consumption and environmental protection is achieved, and the performance of lithium-ion batteries is improved.
Patent Information
- Application Number
- CN202310204582.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-06
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-03-06
AI Technical Summary
The existing NH4V3O8 preparation method requires a high-cost reactor, cumbersome steps, requires acid addition to adjust pH, long hydrothermal time, high energy consumption and not environmentally friendly.
Using the method of automatic pH adjustment, NH4VO3 is stirred and mixed with water and evaporated, the pH of the solution is spontaneously reduced by evaporation of solvent deionized water, and the hydrolysis reaction is realized. Finally, NH4V3O8 powder is obtained by heating and drying, which simplifies the process flow. , reduce energy consumption.
It realizes the preparation of NH4V3O8 without artificial acid addition to adjust pH, shortens reaction time, reduces energy consumption, simplifies equipment and raw materials, is suitable for industrial production, and improves the rate performance and cycle stability of lithium-ion batteries.
Smart Images

Figure CN116375083B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery material preparation, and in particular to a preparation method and application of NH4V3O8 based on automatic pH adjustment. Background Art
[0002] Lithium-ion batteries (LIBs) have become the main energy storage devices in the field of electric vehicles and portable electronic products due to their high energy density, excellent cycle life, no memory effect, and relative environmental protection. In the entire battery system, the positive electrode material plays a vital role. At present, the positive electrode materials that can be used in lithium-ion batteries can be roughly divided into lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium iron phosphate, layered nickel-rich ternary materials, lithium-rich transition metal oxides and vanadium-based materials. Vanadium-based materials have attracted extensive research due to their advantages such as low cost, multiple valence states, large interlayer spacing, and high specific capacity. Ammonium vanadate, as a type of vanadium-based material, has a smaller molecular weight and density than metal vanadates, can form hydrogen bonds between VO layers to enhance structural stability, and NH4 + As pillar ions between VO layers, it has the advantages of avoiding structural damage.
[0003] Existing methods for preparing NH₄V₃O₃ have been reported, including traditional hydrothermal, microwave-assisted, surfactant-assisted, and low-temperature hydrothermal methods. These methods generally require the use of a reactor, which is costly; they are complex and require acid addition for pH control; they undergo long hydrothermal processes (8–48 hours), which is energy-intensive; and some reactions involve the use of organic solvents or the addition of surfactants, which are environmentally unfriendly. Therefore, a novel synthesis method has been proposed to address this issue, eliminating the need for acid addition, enabling automatic pH adjustment, shortening reaction times, and reducing energy consumption. Summary of the Invention
[0004] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a NH4V3O8 preparation method and application based on automatic pH adjustment.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] One of the technical solutions of the present invention is to provide a method for preparing NH4V3O8 based on automatic pH adjustment, comprising the following steps:
[0007] S1. Stirring NH4VO3 and water, and performing evaporation reaction to obtain an orange-yellow powder;
[0008] S2. Heat the orange-yellow powder obtained in step S1 to obtain a reddish-brown powder, which is then dried to obtain NH4V3O8 powder.
[0009] Furthermore, in step S1, the concentration of NH4VO3 after mixing with water is 0.1367 to 0.5470 mol / L.
[0010] Furthermore, in step S1, the stirring time is 8-20 hours.
[0011] Furthermore, in step S1, the process conditions of the evaporation reaction are: the reaction is carried out at a rotation speed of 200-400 rpm and a temperature of 170-300°C.
[0012] Furthermore, in step S1, the evaporation reaction is terminated when the water in the mixed solution of NH4VO3 and water is evaporated to dryness.
[0013] Furthermore, in step S2, the temperature of the heating reaction is 170 to 300° C., and the time of the heating reaction is 10 to 45 minutes.
[0014] Furthermore, in step S2, the drying time is 12 to 24 hours.
[0015] The second technical solution of the present invention is to provide a NH4V3O8, based on the NH4V3O8 preparation method described in one of the above technical solutions.
[0016] The third technical solution of the present invention is to provide an application of NH4V3O8 as described in the second technical solution above, wherein the NH4V3O8 is used as a positive electrode material for preparing a battery.
[0017] Furthermore, the battery is a lithium-ion battery.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] (1) The present invention utilizes the evaporation of deionized water as a solvent to reduce the pH of the mixed solution, thereby realizing a series of hydrolysis reactions that proceed spontaneously using NH4VO3 as a raw material, and finally successfully synthesizing NH4V3O8 powder. The reaction process is as follows: 1. NH4VO3+H2O→HVO3+NH4OH; 2. 4HVO3+H2O→VO3 — +H3O + 3. CH3COOH+H2O→CH3COO — +H3O + ; 4, 2VO3 — +2H + →V2O5+H2O; 5.3V2O5+2NH4OH→2NH4V3O8+H2O. From the above chemical formula, it can be seen that water participates in the reaction and generates H + As water evaporates in the later stage, the acidity of the solution will gradually increase and the pH will decrease. After removing water, the product of the fifth step reaction is NH4V3O8.
[0020] (2) The pH change during the entire process of the present invention can be determined by the color change of the solution. Initially, after heating and dissolving, the solution is a yellow transparent solution. As the water evaporates, the color gradually turns orange-yellow and deepens. Initially, the pH of the solution is about 6. After the water evaporates, it turns into an orange-yellow powder. When the water evaporates to dryness, the pH is about 4, which meets the requirement of adjusting the pH to 2.0-5.5 in the traditional NH4V3O8 preparation method.
[0021] (3) The present invention uses simple equipment, few raw materials, and low cost; the method is simple and does not require manual acid addition to adjust pH; the synthesis time is short and energy consumption is low.
[0022] (4) The present invention has high raw material utilization rate, high yield, can be prepared in large quantities, and is suitable for industrial production.
[0023] (5) The positive electrode material prepared by the present invention was assembled into a lithium ion battery. The experiment showed that the lithium ion battery had excellent rate performance and cycle stability, and achieved high capacity and long life. The battery assembled with the NH4V3O8 positive electrode material synthesized at 230°C had the best performance test, with a capacity of 150mAg. -1 The charge and discharge cycle test was carried out at a current density of 100 cycles, and the specific capacity remained stable at 148.7 mAh g -1 At the same time at 30mAg -1 and 300mAg -1 The specific capacity can reach 415.5mAh g -1 and 135.2mAh g -1 . BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is the XRD pattern of the positive electrode material prepared in Example 1.
[0025] Figure 2 This is the SEM image of the positive electrode material prepared in Example 1.
[0026] Figure 3 This is a comparison chart of the charge and discharge rate performance of the positive electrode materials prepared in Example 1, Example 3 and Example 4 when applied to lithium-ion batteries at different current densities.
[0027] Figure 4 The positive electrode materials prepared in Example 1, Example 3 and Example 4 are applied to lithium ion batteries at a current density of 150 mAg -1 The charge and discharge cycle performance diagram. DETAILED DESCRIPTION
[0028] The present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.
[0029] In the following examples and comparative examples, unless otherwise specified, raw materials or processing techniques are conventional commercially available raw materials or conventional processing techniques in the art.
[0030] Example 1:
[0031] A method for preparing NH4V3O8 based on automatic pH adjustment comprises the following steps:
[0032] Prepare an NH4VO3 solution with a concentration of 0.2735 mol / L (0.8 g NH4VO3 and 25 mL H2O) and magnetically stir for 16 h. Set the stirrer speed to 300 rpm and the temperature to 230°C before heating. After 42 minutes, evaporate the NH4VO3 solution to dryness to form an orange-yellow powder. Continue heating for 20 minutes to form a reddish-brown powder, thus obtaining NH4V3O8.
[0033] Example 2:
[0034] A method for preparing NH4V3O8 based on automatic pH adjustment comprises the following steps:
[0035] Prepare an NH4VO3 solution with a concentration of 0.2735 mol / L (1.6 g NH4VO3 and 50 mL H2O) and magnetically stir for 20 h. Set the stirrer speed to 300 rpm and the temperature to 230°C before heating. After 90 min, evaporate the solution to dryness to form an orange-yellow powder. Continue heating for 25 min to form a reddish-brown powder, thus obtaining NH4V3O8.
[0036] Example 3:
[0037] A method for preparing NH4V3O8 based on automatic pH adjustment comprises the following steps:
[0038] Prepare an NH4VO3 solution with a concentration of 0.2735 mol / L (0.8 g NH4VO3 and 25 mL H2O) and magnetically stir for 16 h. Set the stirrer speed to 300 rpm and the temperature to 260°C before heating. After 35 min, evaporate the solution to dryness to form an orange-yellow powder. Continue heating for 16 min to form a reddish-brown powder, thus obtaining NH4V3O8.
[0039] Example 4:
[0040] Prepare an NH4VO3 solution with a concentration of 0.2735 mol / L (0.8 g NH4VO3 and 25 mL H2O) and stir magnetically for 16 h. Set the stirrer speed to 300 rpm and the temperature to 200°C before heating. After 54 min, evaporate the solution to dryness to form an orange-yellow powder. Continue heating for 40 min to form a reddish-brown powder, thus obtaining NH4V3O8.
[0041] Example 5:
[0042] Prepare an NH4VO3 solution with a concentration of 0.1367 mol / L (0.4 g NH4VO3 and 25 mL H2O) and stir magnetically for 8 h. Set the stirrer speed to 300 rpm and the temperature to 230°C before heating. After 42 min, evaporate the solution to dryness to form an orange-yellow powder. Continue heating for 15 min to form a reddish-brown powder, thus obtaining NH4V3O8.
[0043] Example 6:
[0044] Prepare an NH4VO3 solution with a concentration of 0.5470 mol / L (1.6 g NH4VO3 and 25 mL H2O) and magnetically stir for 20 h. Set the stirrer speed to 400 rpm and the temperature to 230°C before heating. After 42 minutes, evaporate the solution to dryness to form an orange-yellow powder. Continue heating for 32 minutes to form a reddish-brown powder, thus obtaining NH4V3O8.
[0045] The NH4V3O8 prepared in the above example was used as the positive electrode material to assemble a battery. There were no particular restrictions on the types of electrodes, separators, and electrolytes. The electrodes used lithium sheets, the separators used polypropylene films, and the electrolyte used a mixture of EC, DEC, and EMC. Specifically, the NH4V3O8 powdered positive electrode material was formed into electrode sheets using a conventional slurry coating method. A lithium sheet was used as the negative electrode. 1M LiPF6 was dissolved in a 1:1:1 volume ratio of EC, DEC, and EMC, and 1% FEC was added as the electrolyte. Celgard 2600 microporous polypropylene membrane served as the separator, and the battery was assembled into a CR2016 model battery.
[0046] Using 150mAg -1 The constant current charge and discharge experiments were conducted to test the cycle performance of the lithium-ion battery, with the charge and discharge voltage limited to 1.5 to 3.2 V. The electrochemical performance of the battery was tested using the CT2001A battery test system from Wuhan Blue Electric Electronics Co., Ltd. at room temperature.
[0047] Here are the results:
[0048] like Figure 11 is the XRD pattern of the NH4V3O8 powder prepared in Example 1, and the characteristic peaks correspond to the standard card JCPDS: 88-1473.
[0049] like Figure 2 As shown, it is a scanning electron microscope image of the NH4V3O8 powder prepared in Example 1. It can be seen that the morphology of NH4V3O8 is a nanosheet structure.
[0050] like Figure 3 As shown in the figure, the rate performance of the battery assembled with the electrode sheet made of the NH4V3O8 powder coating prepared in Examples 1, 3, and 4 was tested for charge and discharge cycle. The material synthesized at 230℃ (Example 1) had the best performance and -1 and 300mAg -1 The specific capacity can reach 415.5mAh g -1 and 135.2mAh g -1 .
[0051] like Figure 4 As shown in the figure, the cycle performance test results of the battery assembled with the electrode sheet made of the NH4V3O8 powder coating prepared in Examples 1, 3, and 4 for charge and discharge cycle test are shown in the figure. -1 The charge-discharge cycle test was carried out at a current density of 230 ° C. The material synthesized at 230 ° C (Example 1) maintained a stable specific capacity of 148.7 mAh g after 100 cycles. -1 .
[0052] In summary, the concentration of the preferably prepared NH4VO3 solution is 0.2735 mol / L (0.8 g NH4VO3 and 25 mL H2O), the stirring time is preferably 16 h, the speed of the magnetic stirrer is set to 300 rpm, the evaporation reaction temperature is preferably 230 ° C, the time to form an orange-yellow powder is preferably 35 to 45 min, and the time to continue the evaporation reaction until a reddish-brown powder is formed is preferably 15 to 30 min.
[0053] The battery performance test of the NH4V3O8 cathode material synthesized at an evaporation temperature of 230℃ was the best, with a -1 The charge and discharge cycle test was carried out at a current density of 100 cycles, and the specific capacity remained stable at 148.7 mAh g -1 At the same time at 30mAg -1 and 300mAg -1 The specific capacity can reach 415.5mAh g -1 and 135.2mAhg -1 , with excellent rate performance and cycle stability.
[0054] The above description of the embodiments is intended to facilitate understanding and use of the invention by those skilled in the art. It will be apparent that those skilled in the art can readily make various modifications to these embodiments and apply the general principles described herein to other embodiments without requiring inventive effort. Therefore, the present invention is not limited to the above-described embodiments. Improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing NH4V3O8 based on automatic pH adjustment, characterized in that: The steps include: S1. Stir and mix NH4VO3 and water, and evaporate them to obtain an orange-yellow powder; S2, heating the orange-yellow powder obtained in step S1 to obtain a reddish-brown powder, which is dried to obtain NH4V3O8 powder; In step S1, the concentration of NH4VO3 after mixing with water is 0.1367-0.5470 mol / L, and the process conditions of the evaporation reaction are: the reaction is carried out at a rotation speed of 200-400 rpm and a temperature of 230-260 °C, and the evaporation reaction is terminated when the water in the mixed solution of NH4VO3 and water is evaporated; In step S2, the heating reaction temperature is 230-260°C, and the heating reaction time is 10 to 45 min.
2. The method for preparing NH4V3O8 based on automatic pH adjustment according to claim 1, characterized in that: In step S1, the stirring time is 8-20 h.
3. The method for preparing NH4V3O8 based on automatic pH adjustment according to claim 1, characterized in that: In step S2, the drying time is 12 to 24 h.