Method for preparing enamel non-stick material, enamel non-stick material and cookware
By using a mixed material of calcium sulfate whiskers and enamel materials in the enamel coating, the network structure is formed, which solves the problems of poor non-stickness and fragility of the enamel coating, improves the strength and non-stick properties of the pot, and achieves aesthetics Durable effect.
Patent Information
- Application Number
- CN202211701737.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-12-28
AI Technical Summary
The non-stickness of the enamel coating is poor, fragile, and locally heated and explosive porcelain, making it difficult to improve its strength and non-stick properties while maintaining its beauty and durability and improving metal corrosion resistance.
The mixed material of calcium sulfate whiskers and enamel material is used to uniformly disperse the calcium sulfate whiskers in the enamel material through melting and cold quenching, forming a network structure, filling the gaps of the enamel non-stick coating, and improving its strength and non-stick properties.
It significantly improves the strength, wear resistance and non-stick properties of the enamel non-stick coating, enhances its oil absorption characteristics, and ensures the long-lasting non-stickness and impact resistance of the pan.
Smart Images

Figure BDA0004024233500000071 
Figure BDA0004024233500000081
Abstract
Description
Technical Field
[0001] The present invention relates to the field of cookware, and more particularly to a method for preparing a non-stick enamel material, the non-stick enamel material prepared by the method, and a cookware comprising the non-stick enamel material. Background Art
[0002] Enamel is an inorganic glassy material. In recent years, enamel coatings have been prepared by melting and solidifying inorganic glassy materials on metal substrates. Enamel coatings can protect metals, prevent them from rusting, and improve the corrosion resistance of metals. At the same time, enamel coatings have the characteristics of being beautiful and durable. However, enamel coatings have poor non-stick properties, are fragile, and are prone to cracking due to local heating. Summary of the invention
[0003] In order to solve the above technical problems, the purpose of the present invention is to provide a method for preparing a non-stick enamel material and a non-stick enamel material prepared by the method. The present invention uses a mixed material of calcium sulfate whiskers and enamel materials to prepare a non-stick enamel material for cookware. In the non-stick enamel coating prepared thereby, the calcium sulfate whiskers can be dispersed therein and form a network structure to fill the gaps in the non-stick enamel coating and improve the strength of the non-stick enamel coating; at the same time, the network structure formed by the calcium sulfate whiskers improves its oil absorption characteristics and increases the non-stick performance of the non-stick enamel coating.
[0004] According to one aspect of the present invention, a method for preparing a non-stick enamel material comprises: mixing a enamel material and a calcium sulfate whisker and then melting them so that the enamel material, but not the calcium sulfate whisker, is in a molten state; cold quenching the molten material to obtain a mixture in which the calcium sulfate whisker is dispersed in the molten enamel material; and ball milling the mixture to obtain a non-stick enamel material with a predetermined particle size, wherein the calcium sulfate whisker accounts for 0.5wt% to 1wt% based on the total weight of the non-stick enamel material. Through the above preparation method, the calcium sulfate whisker can be evenly dispersed in the enamel material, which facilitates the subsequent formation of a network structure by the calcium sulfate whisker.
[0005] In an embodiment of the present invention, the enamel material and the calcium sulfate whiskers can be melted at a temperature of 1100-1200° C. At a temperature of 1100-1200° C., the enamel material can be melted, while the calcium sulfate whiskers are not melted, so the unmelted calcium sulfate whiskers can be uniformly dispersed in the molten enamel material.
[0006] In an embodiment of the present invention, the calcium sulfate whiskers may include anhydrous calcium sulfate whiskers, and the enamel material may include silicates. Anhydrous calcium sulfate whiskers are more stable at high temperatures. Silicates (including borosilicates) can protect metals from rust and improve the corrosion resistance of metals.
[0007] In an embodiment of the present invention, in the step of ball milling the mixture, the mixture may be ball milled for 90 to 110 hours, and the ball milled mixture may be sieved to obtain an enamel non-stick material with a particle size of 20 to 30 μm. The enamel non-stick material within the above particle size range can prepare an enamel non-stick coating with good gloss.
[0008] In an embodiment of the present invention, the calcium sulfate whisker may have a diameter of 1-5 μm, a length of 50-100 μm, and an aspect ratio of 10-100.
[0009] In an embodiment of the present invention, the calcium sulfate whisker may have a tensile strength of 16-25 GPa and a tensile modulus of 170-180 GPa. The calcium sulfate whisker with high tensile strength and high tensile modulus plays a protective role on the enamel non-stick coating.
[0010] According to one aspect of the present invention, an enamel non-stick material comprises a enamel material and calcium sulfate whiskers dispersed in the enamel material, wherein the calcium sulfate whiskers account for 0.5wt% to 1wt% based on the total weight of the enamel non-stick material. The enamel non-stick coating prepared from the enamel non-stick material has good non-stick properties and impact resistance.
[0011] In an embodiment of the present invention, the calcium sulfate whiskers may include anhydrous calcium sulfate whiskers, and the enamel material may include silicates. Anhydrous calcium sulfate whiskers are more stable at high temperatures. Silicates (including borosilicates) can protect metals from rust and improve the corrosion resistance of metals.
[0012] In an embodiment of the present invention, the silicate may include at least one of quartz, feldspar and borax.
[0013] According to one aspect of the present invention, the cookware comprises a metal substrate and an enamel non-stick coating on the metal substrate, wherein the enamel non-stick coating comprises an enamel non-stick material, and wherein calcium sulfate whiskers form a network structure in the enamel non-stick coating. The calcium sulfate whiskers can fill the voids in the enamel non-stick coating and improve the strength of the enamel non-stick coating; at the same time, the network structure formed by the calcium sulfate whiskers improves its oil absorption characteristics and increases the non-stick performance of the enamel non-stick coating.
[0014] The enamel non-stick coating prepared from the enamel non-stick material according to the embodiment has enhanced strength and wear resistance due to the addition of calcium sulfate whiskers, and has good non-stick and long-lasting non-stick properties. DETAILED DESCRIPTION
[0015] Now, the present invention will be more fully described below in conjunction with exemplary embodiments. However, the present invention can be implemented in a variety of different forms and should not be construed as being limited to the exemplary embodiments set forth herein. These embodiments are provided so that the disclosure of the present invention will be thorough and complete, and the scope of the present invention will be fully conveyed to those skilled in the art.
[0016] Enamel is an inorganic glassy material. The enamel coating is prepared by melting and solidifying the inorganic glassy material (enamel) on a metal substrate. The enamel coating can protect the metal from rust and improve the corrosion resistance of the metal. At the same time, the enamel coating has the characteristics of beauty and durability.
[0017] Calcium sulfate whisker is a new type of needle-shaped fiber sub-nano material grown in the form of single crystal, with uniform cross-section, complete appearance and perfect internal structure. Compared with other short fibers, calcium sulfate whisker has the advantages of high temperature resistance, chemical corrosion resistance, good toughness, high strength and easy surface treatment. The calcium sulfate whisker used in the present invention is a fibrous single crystal of anhydrous calcium sulfate.
[0018] According to an embodiment of the present invention, the enamel non-stick material may include a enamel material and calcium sulfate whiskers uniformly dispersed in the enamel material. Based on the total weight of the enamel non-stick material, the calcium sulfate whiskers may account for 0.5wt% to 1wt% (e.g., 0.6wt% to 1wt%, 0.7wt% to 1wt%, 0.8wt% to 1wt% or 0.9wt% to 1wt% or any range of the above given values).
[0019] In an embodiment of the present invention, if the calcium sulfate whisker accounts for more than 1wt%, in the enamel non-stick coating prepared from the enamel non-stick material, the surface roughness of the enamel non-stick coating will be reduced due to excessive addition of calcium sulfate whiskers, which will reduce its color, and the enamel non-stick coating will present a matte effect; and too much calcium sulfate whiskers may even cause appearance defects on the surface of the enamel non-stick coating, such as concave and convex particles, cracks, peeling and pinholes. In addition, too much calcium sulfate whiskers will also reduce the non-stick performance of the enamel non-stick coating. If the calcium sulfate whisker accounts for less than 0.5wt%, in the enamel non-stick coating prepared from the enamel non-stick material, the calcium sulfate whiskers cannot form a network structure, resulting in the enamel non-stick coating having poor performance in terms of non-stickiness, durable non-stickiness and strength.
[0020] In an embodiment of the present invention, the calcium sulfate whisker may include or be anhydrous calcium sulfate whisker. Anhydrous calcium sulfate whisker is more stable at high temperatures. The calcium sulfate whisker may have a tensile strength of 16-25 Gpa (e.g., 18-24 Gpa, 20-22 Gpa, or 20.5 Gpa) and a tensile modulus of 170-180 Gpa (e.g., 172-179 Gpa or 178 Gpa).
[0021] According to an embodiment of the present invention, the enamel material may include a silicate. The silicate may include a borosilicate. Examples of silicates may include at least one of quartz, feldspar and borax. Silicates (including borosilicates) can protect metals, prevent them from rusting, and improve the corrosion resistance of metals. In an embodiment of the invention, the enamel material may also include other additives. For example, the enamel material may also include a fluxing agent that can promote its melting to improve processing performance and a colorant that changes its color.
[0022] Hereinafter, a method for preparing the enamel non-stick material will be described in detail.
[0023] The method for preparing a non-stick enamel material may include: mixing a enamel material and a calcium sulfate whisker and then melting them so that the enamel material, but not the calcium sulfate whisker, is in a molten state; quenching the molten material to obtain a mixture in which the calcium sulfate whisker is dispersed in the molten enamel material; and ball milling the mixture to obtain a non-stick enamel material with a predetermined particle size. During the preparation process, the calcium sulfate whisker may account for 0.5wt% to 1wt% based on the total weight of the non-stick enamel material.
[0024] In an embodiment of the present invention, the calcium sulfate whisker may include or be anhydrous calcium sulfate whisker. Anhydrous calcium sulfate whisker is more stable at high temperatures. For example, anhydrous calcium sulfate whisker can stably exist in the subsequent sintering process for preparing enamel non-stick coating. The calcium sulfate whisker can have a diameter of 1 to 5 μm, a length of 50 to 100 μm (e.g., 60 to 90 μm or 70 to 80 μm), and an aspect ratio of 10 to 100 (e.g., 20 to 90, 30 to 80, 40 to 70, and 50 to 60). The enamel material is the same as the enamel material described above.
[0025] In an embodiment of the present invention, the enamel material and the calcium sulfate whiskers can be fully melted in a box furnace at a temperature of 1100-1200° C., so that the calcium sulfate whiskers are uniformly dispersed in the enamel material. At a temperature of 1100-1200° C., the enamel material is in a molten state, while the calcium sulfate whiskers are not melted. In this case, the unmelted calcium sulfate whiskers can be uniformly dispersed in the molten enamel material.
[0026] According to an embodiment of the present invention, in the step of quenching the molten material, the molten material may be placed in cold water for quenching.
[0027] In an embodiment of the present invention, the cold-quenched mixture can be ball-milled for 90 to 110 hours, and then the ball-milled mixture can be sieved to obtain an enamel non-stick material with a particle size of 20 to 30 μm (for example, 22 to 28 μm or 24 to 26 μm). The calcium sulfate whiskers after ball milling will break, and the broken calcium sulfate whiskers will be evenly dispersed in the enamel non-stick material. The finer the particle size of the enamel non-stick material, the brighter the gloss of the enamel non-stick coating prepared therefrom. However, if the particle size of the enamel non-stick material is too fine, it will easily lead to the generation of cracks. Therefore, the particle size of the enamel non-stick material is controlled within the range of 20-30 μm.
[0028] Calcium sulfate whiskers with a particle size close to that of the enamel non-stick material after ball milling have better dispersibility in the enamel material. For example, the calcium sulfate whiskers preferably have a length of 30-70 μm. If the length of the calcium sulfate whiskers is too small, it is difficult to ensure that a network structure is formed in the enamel non-stick coating prepared subsequently.
[0029] The preparation method of the above-mentioned enamel non-stick material can ensure the dispersibility of calcium sulfate whiskers in the enamel material, thereby ensuring that the calcium sulfate whiskers can be distributed and run through the entire enamel non-stick coating prepared in the subsequent process, so that they can form a network structure in the enamel non-stick coating.
[0030] In an embodiment of the present application, the cookware may include a metal substrate and an enamel non-stick coating on the metal substrate, wherein the enamel non-stick coating may include the above-mentioned enamel non-stick material, and the calcium sulfate whiskers may form a network structure in the enamel non-stick coating.
[0031] In the enamel non-stick coating according to the embodiment, the calcium sulfate whiskers can form a network structure therein, fill the gaps in the enamel non-stick coating, and improve the strength of the enamel non-stick coating; at the same time, the network structure formed by the calcium sulfate whiskers improves the oil absorption characteristics of the enamel non-stick coating and increases the non-stick performance of the enamel non-stick coating.
[0032] In addition, when the enamel non-stick coating according to the embodiment is subjected to impact or wear, the calcium sulfate whiskers with high tensile strength (16-25GPa) and high tensile modulus (170-180GPa) can protect the enamel non-stick coating, enhance the strength and wear resistance of the enamel non-stick coating, and improve the non-stickiness and long-lasting non-stickness of the enamel non-stick coating.
[0033] According to an embodiment of the present invention, a method for preparing a cookware may include the following steps: mixing the enamel non-stick material prepared by the above method with water to prepare a slurry with a solid content of 50wt%-70wt%; spraying the slurry on a metal substrate; and sintering the metal substrate sprayed with the slurry to prepare a cookware including a enamel non-stick coating.
[0034] According to an embodiment of the present invention, the slurry can be sprayed on the metal substrate in a spraying manner. In addition, the metal substrate sprayed with the slurry can be sintered at a temperature of 850 to 950° C. The gas generated during the sintering process can be discharged to the outside of the enamel non-stick coating along the calcium sulfate whiskers in the enamel non-stick coating, reducing the porosity of the enamel non-stick coating, thereby improving the strength of the enamel non-stick coating. The enamel non-stick coating according to an embodiment of the present invention has enhanced strength and wear resistance due to the addition of calcium sulfate whiskers, and has good non-stick and long-lasting non-stick properties.
[0035] The method for preparing the enamel non-stick coating of the present invention will be described in detail below with reference to examples.
[0036] Example 1
[0037] Calcium sulfate whiskers and quartz are fully mixed (wherein, the content of calcium sulfate whiskers is 0.5wt% based on the total weight of the enamel non-stick material; and wherein, the average diameter of the calcium sulfate whiskers is 2μm and the average length is 50μm), and then melted in a box furnace at a temperature of 1100°C. The molten material is poured into cold water and quenched into a mixture. The mixture is broken, ball-milled for 100h, and sieved to obtain an enamel non-stick material with an average particle size of 20μm. The prepared non-stick coating is mixed with water to prepare a slurry with a solid content of 60wt%. The slurry is sprayed on the surface of the cast iron pot embryo by spraying, and then sintered at a temperature of 900°C to prepare a pot including an enamel non-stick coating.
[0038] Example 2
[0039] The cookware according to Example 2 was manufactured in the same manner as in Example 1, except that the content of the calcium sulfate whisker was 0.6 wt % based on the total weight of the enamel non-stick material.
[0040] Example 3
[0041] The cookware according to Example 3 was manufactured in the same manner as in Example 1, except that the content of the calcium sulfate whisker was 0.8 wt % based on the total weight of the enamel non-stick material.
[0042] Example 4
[0043] The cookware according to Example 4 was manufactured in the same manner as in Example 1, except that the content of the calcium sulfate whisker was 1.0 wt % based on the total weight of the enamel non-stick material.
[0044] Example 5
[0045] The cookware according to Example 5 was manufactured in the same manner as in Example 1, except that the average length of the calcium sulfate whiskers was 70 μm.
[0046] Example 6
[0047] The cookware according to Example 6 was manufactured in the same manner as in Example 1, except that the average length of the calcium sulfate whiskers was 100 μm.
[0048] Example 7
[0049] The cookware according to Example 7 was manufactured in the same manner as in Example 1, except that the enamel non-stick material having an average particle size of 30 μm was used.
[0050] Comparative Example 1
[0051] The cookware according to Comparative Example 1 was manufactured using the same method as that of Example 1, except that the calcium sulfate whiskers were not added.
[0052] Comparative Example 2
[0053] The cookware according to Comparative Example 2 was manufactured in the same method as that of Example 1, except that the content of the calcium sulfate whisker was 0.3 wt % based on the total weight of the enamel non-stick material.
[0054] Comparison Example 3
[0055] The cookware according to Comparative Example 3 was manufactured in the same method as that of Example 1, except that the content of the calcium sulfate whisker was 2 wt % based on the total weight of the enamel non-stick material.
[0056] Comparison Example 4
[0057] The cookware according to Comparative Example 5 was manufactured in the same method as that of Example 1, except that the average particle size of the enamel non-stick material after ball milling was 40 μm.
[0058] Comparative Example 5
[0059] The cookware according to Comparative Example 6 was manufactured in the same method as that of Example 1, except that the average particle size of the enamel non-stick material after ball milling was 15 μm.
[0060] The enamel non-stick coatings of the cookware according to Examples 1 to 7 and Comparative Examples 1 to 5 were subjected to a non-stick test, a long-lasting non-stick test, and an impact resistance test.
[0061] (1) Non-stick test
[0062] The test was conducted with reference to the non-stickiness test of fried eggs in 4.2.1 of GB_T32095.2-2015. Specifically, (1) Pour an appropriate amount of vegetable oil into the cooking utensil and wipe the non-stick surface with a soft cloth until the coating is evenly applied; (2) Wash with warm water above 60°C and neutral detergent, then rinse with clean water and wipe dry; (3) Heat the cooking utensil on an electric stove with a rated voltage of 220V and an output power of 1kW, and measure with a surface thermometer with an accuracy of not less than 2.5 levels. When the surface temperature of the inner coating reaches 150-170°C, break a fresh egg that meets the requirements of SB / T10277-1997, level 2 (weight 50-60g), and place it into the cooking utensil until the egg white is basically coagulated (during the entire cooking process, the surface temperature of the inner coating shall not exceed 210°C); (4) Take out the egg intact with a plastic spatula with a cutting edge thickness of 0.2-0.5mm. If egg residue remains, wipe it off gently with a wet sponge or gauze; (5) Repeat steps (3) and (4) three times in total and observe.
[0063] (2) Long-lasting non-stick test
[0064] Refer to the plane wear resistance test of GB_T32095.2-2015 for testing. When the number of cycles is equal to one thousand times, the fried egg non-stick test of 4.2.1 is carried out to test the non-stickiness. Specifically, (1) After cleaning the cooking utensils, fix them on the wear resistance test machine, at a frequency of 33 times / min, apply a downward force of 15N, use a scouring pad (3M7447B) with a length of 70mm±5mm and a width of 30mm±5mm, and move back and forth for a distance of 100mm; (2) Start the test machine, replace the scouring pad every 500 times and observe with a 10x magnifying glass. If the non-stick surface has a wear mark with a width of more than 1mm on the exposed substrate or 10 linear wear marks with a length of more than 2mm on the exposed substrate, stop the test; (3) Record the number of cycles N, which shall be based on the total number of cycles before the test is terminated.
[0065] (3) Impact resistance test
[0066] Refer to 6.2.3 of GB / T13484-2011 for testing. Specifically, place the sample in the state of use, use two wooden pads to support the two ends of the bottom of the sample, and make the bottom of the sample more than 30mm from the bottom surface. Use a 200g steel ball to freely fall at 1800mm (the distance between the center of the steel ball and the test surface of the sample) to impact the bottom of the sample, and observe the porcelain surface after 24 hours.
[0067] The test results are shown in Table 1 below.
[0068] Table 1
[0069]
[0070]
[0071] By comparing Examples 1 to 7 of the present invention with Comparative Examples 1 to 5, it can be seen that the enamel non-stick coating according to the present invention has good non-stick properties and durable non-stick properties, and has excellent impact resistance.
[0072] In combination with Examples 1 to 4 and Comparative Examples 1 to 3, it can be seen that the addition of calcium sulfate whiskers and the amount of calcium sulfate whiskers added have an important influence on the performance of the enamel non-stick coating. In the case where calcium sulfate whiskers are not added to the enamel non-stick coating (i.e., Comparative Example 1), the enamel non-stick coating exhibits poor performance in terms of non-stickiness, lasting non-stickiness and impact resistance. In the case where the addition amount of calcium sulfate whiskers is 0.3wt% (i.e., Comparative Example 2), due to the small amount of addition, the non-stickiness, lasting non-stickiness and impact resistance of the enamel non-stick coating are not good. In the case where the addition amount of calcium sulfate whiskers is 2wt% (i.e., Comparative Example 3), due to the excessive amount of addition, the non-stickiness and lasting non-stickiness of the enamel non-stick coating are deteriorated.
[0073] When the average particle size of the enamel non-stick material is 40 μm (i.e., Comparative Example 4), the average particle size of the enamel non-stick material is too large, resulting in a dull and dull porcelain surface of the formed enamel non-stick coating, which affects the appearance of the cookware. When the average particle size of the enamel non-stick material is 15 μm (i.e., Comparative Example 5), the average particle size of the enamel non-stick material is too small, resulting in cracks on the porcelain surface of the formed enamel non-stick coating, which affects the use effect.
[0074] A mixed material of calcium sulfate whiskers and enamel materials is used to prepare an enamel non-stick coating for cookware. In the prepared enamel non-stick coating, the calcium sulfate whiskers can be dispersed therein and form a network structure to fill the gaps in the enamel non-stick coating and improve the strength of the enamel non-stick coating; at the same time, the network structure formed by the calcium sulfate whiskers improves its oil absorption characteristics and increases the non-stick performance of the enamel non-stick coating.
[0075] Although the present invention has been specifically shown and described with reference to exemplary embodiments of the present invention, it will be understood by those skilled in the art that various changes in form and detail may be made herein without departing from the spirit and scope of the present invention as defined by the claims and their equivalents. The embodiments should be considered in a descriptive sense only and not for the purpose of limitation. Therefore, the scope of the present invention is not limited by the specific embodiments of the present invention, but by the claims, and all differences within the scope will be interpreted as included in the present invention.
Claims
1. A method for preparing an enamel non-stick material, characterized in that: The method comprises the following steps: The enamel material and the calcium sulfate whisker are mixed and then melted so that the enamel material but not the calcium sulfate whisker is in a molten state; quenching the molten material to obtain a mixture in which calcium sulfate whiskers are dispersed in the molten enamel material; and The mixed material is ball-milled to obtain an enamel non-stick material with a predetermined particle size. Wherein, based on the total weight of the enamel non-stick material, the calcium sulfate whisker accounts for 0.5wt% to 1wt%.
2. The method according to claim 1, characterized in that The enamel material and the calcium sulfate whisker are melted at a temperature of 1100-1200°C.
3. The method according to claim 1, characterized in that Calcium sulfate whiskers include anhydrous calcium sulfate whiskers, Enamel materials include silicates.
4. The method according to claim 1, characterized in that: In the step of ball-milling the mixed material, the mixed material is ball-milled for 90 to 110 hours, and the ball-milled mixed material is sieved to obtain an enamel non-stick material with a particle size of 20 to 30 μm.
5. The method according to claim 1, characterized in that The calcium sulfate whiskers have a diameter of 1-5 μm, a length of 50-100 μm, and an aspect ratio of 10-100.
6. The method according to claim 1, characterized in that Calcium sulfate whiskers have a tensile strength of 16-25 GPa and a tensile modulus of 170-180 GPa.
7. An enamel non-stick material prepared by the method of claim 1, characterized in that: The enamel non-stick material comprises a enamel material and calcium sulfate whiskers dispersed in the enamel material. Wherein, based on the total weight of the enamel non-stick material, the calcium sulfate whisker accounts for 0.5wt% to 1wt%.
8. The enamel non-stick material according to claim 7, characterized in that: Calcium sulfate whiskers include anhydrous calcium sulfate whiskers, Enamel materials include silicates.
9. The enamel non-stick material according to claim 8, characterized in that: The silicate includes at least one of quartz, feldspar and borax.
10. A cookware, characterized in that: The cookware comprises a metal substrate and an enamel non-stick coating on the metal substrate. wherein the enamel non-stick coating comprises the enamel non-stick material according to any one of claims 7 to 9, and Among them, calcium sulfate whiskers form a network structure in the enamel non-stick coating.
Citation Information
Patent Citations
High temperature super wear-resisting non-sticking graphene coating material
CN107841205A
Silky fine matt ceramic tile and production method thereof
CN110204306A
High-strength crackle glaze, high-strength crackle glaze ceramic product and preparation method of high-strength crackle glaze ceramic product
CN113024282A
Digital carving ceramic and preparation method thereof
CN113105116A
Glaze layer slurry, sanitary ceramics with smooth surface and ceramic preparation method
CN113135661A