An organic Janus nanosheet-stabilized water-based carbon dioxide foam and its preparation method and application
Patent Information
- Application Number
- CN202310017710.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-01-06
AI Technical Summary
Existing technology is difficult to effectively stabilize CO2 foam, resulting in gravity differentiation and fingering of CO2 during formation flow, which reduces storage efficiency and quantity. In particular, two-dimensional nanoparticles have poor stability at the air-water interface and are difficult to inhibit CO2 diffusion. .
Organic Janus nanosheets are used to form a dense nano-armor layer through the uniform distribution of hydrophobic and hydrophilic groups to inhibit CO2 diffusion and improve foam stability. By controlling the size and morphology of the nanosheets, the interface viscoelasticity is enhanced to control CO2 Fluidity.
The ultra-stable water-based CO2 foam has been realized, which enhances the storage safety and geological storage capacity of CO2. By forming an efficient nano-armor layer, it inhibits the flow of CO2 and expands the scope of CO2 storage.
Abstract
Description
Technical Field
[0001] This invention relates to an organic Janus nanosheet-stabilized water-based carbon dioxide foam, its preparation method and application, belonging to the fields of nanomaterial preparation technology and carbon sequestration and utilization technology. Background Technology
[0002] Fossil fuels are one of the world's main sources of energy supply. However, with the continuous growth of social demand, the large-scale consumption of fossil fuels has exacerbated the emission of greenhouse gases such as CO2. Excessive CO2 emissions into the atmosphere have led to rising global temperatures and drastic climate change. How to reduce atmospheric CO2 concentration has received widespread attention and importance worldwide. Carbon capture, utilization, and storage (CCUS) technology is considered one of the most effective solutions for reducing atmospheric CO2 concentration. Injecting CO2 into formations is currently one of the most promising methods for large-scale CO2 storage, such as injecting it into deep saline aquifers, abandoned oil and gas reservoirs, coal seams, and for enhanced oil and gas recovery. However, because CO2 has a much lower viscosity and density than oil and water, and a higher mobility, it is prone to gravity differentiation and fingering during formation flow, resulting in low sweep efficiency and low storage capacity.
[0003] Foam is a multiphase fluid with high viscosity. During flow in porous media, it exhibits the Jamin effect, increasing flow resistance and reducing gas mobility, thus making it a highly efficient system for controlling flowability. However, foam is a thermodynamically unstable system; behaviors such as separation, coalescence, and rupture weaken its effectiveness. Based on Pickering theory, the adsorption of nanoparticles on the foam surface can improve foam stability. Numerous studies have demonstrated that nanoparticle-surfactant systems can prepare homogeneous foams with higher viscosity, exhibiting stronger flowability control than foams prepared from pure surfactant solutions. Nanoparticle-reinforced foams, due to their high Jamin resistance and wall friction resistance, can control fluid flow direction and improve sweep efficiency.
[0004] Based on particle size and aspect ratio, nanoparticles can be mainly divided into three categories: zero-dimensional nanoparticles, one-dimensional nanoparticles (such as nanowires), and two-dimensional nanoparticles (such as nanosheets). Zero-dimensional nanoparticles are mainly spherical, and commonly used material substrates include oxides of elements such as Si, Ti, Fe, and Al. Their bubble stabilization mechanism mainly involves adsorbing at the gas-liquid interface and Plateau boundary of the foam, reducing the contact area between bubbles, forming a dense particle film to inhibit bubble aggregation and disproportionation, prolonging the liquid film drainage time, and improving the strength of the liquid film skeleton. In addition, nanoparticles can improve the viscoelasticity of the liquid film interface, enhancing the self-recovery ability of the liquid film when subjected to external impact. However, due to the morphological characteristics of zero-dimensional nanomaterials, they are partially stacked and adsorbed on the liquid film surface, which easily leads to slippage, thus limiting the effect of slowing down aggregation. Furthermore, compared with air or nitrogen, CO2 has stronger diffusion, and CO2 foam has poorer stability. Spherical zero-dimensional nanomaterials have small aspect ratios and dimensions, requiring a larger quantity to form a nano-reinforced film at the gas-liquid interface. Furthermore, the large gaps between particles limit their ability to inhibit CO2 diffusion. One-dimensional nanoparticles primarily improve foam stability by forming a network structure within the liquid film to increase the viscosity of the liquid phase, thereby inhibiting film thinning due to liquid separation. On the other hand, one-dimensional nanoparticles can promote a more compact arrangement of surfactant molecules at the interface, increasing the difficulty of gas permeation through the liquid film and thus slowing down bubble aggregation and disproportionation. However, one-dimensional nanoparticles also have significant drawbacks: the mechanical strength of the liquid film cannot be effectively enhanced, and their distribution on the liquid film surface is generally uneven. At slightly higher concentrations, they are prone to entanglement and aggregation into large polymer molecules, making it difficult to maintain stability at the phase interface. Additionally, similar to zero-dimensional nanoparticles, one-dimensional nanoparticles still require the adsorption of a large number of particles to stabilize CO2 foam, increasing costs.
[0005] Based on the aforementioned issues, two-dimensional nanoparticles have attracted attention for stabilizing phase interfaces. Firstly, from a morphological perspective, compared to zero-dimensional and one-dimensional nanoparticles, two-dimensional nanoparticles, due to their unique sheet-like morphology and larger aspect ratio, possess a greater potential for stable adsorption at phase interfaces. This allows them to form an interfacial armor film at the interface, which is less prone to detachment, requires smaller quantities, and has smaller gaps between nanosheets, limiting mass transfer between bubbles and thus exhibiting stronger potential for inhibiting CO2 diffusion between bubbles. Secondly, based on adsorption energy, it is known that two-dimensional nanosheets are difficult to effectively adsorb onto the surface of emulsions or bubbles to improve stability, mainly due to the influence of the hydrophilic / hydrophobic properties and size control of the nanosheets. Benefiting from the dual-sided nature of nanosheets, inspired by the molecular structure of surfactants, two-dimensional nanosheets can be endowed with hydrophilic and hydrophobic properties on both sides, acquiring diametrically opposed properties, i.e., Janus properties. This allows Janus particles to spontaneously tend towards the phase interface, forming a stable reinforcing layer for emulsions or foams. Currently, two-dimensional Janus nanosheets are commonly used to prepare Pickering emulsions, demonstrating significant application value in cosmetics, construction, and pharmaceutical industries. However, compared to the oil-water interface, the gas-water interface of foam exhibits greater interfacial tension and more intense gas diffusion, especially with CO2 gas. Therefore, stabilizing the gas-water interface is more challenging, and there are few reports on Janus nanosheets stabilizing foams. The strong instability of foams poses a significant challenge to the hydrophilic-hydrophobic balance and the compact adsorption size of Janus nanosheets. Therefore, a method is needed to achieve low-cost, mild-condition synthesis of Janus nanosheets, which can be used to tightly coat foam surfaces to form ultra-stable water-based CO2 foams. This would effectively control the mobility of CO2 during transport in porous media, improving CO2 sequestration safety and geological sequestration capacity. Summary of the Invention
[0006] The purpose of this invention is to provide an organic Janus nanosheet-stabilized water-based carbon dioxide foam. The two-dimensional organic Janus nanosheets exhibit uniform distribution of amphiphilic groups, strong Janus properties, controllable nanosheet size, and simple synthesis. The two-dimensional organic Janus nanosheets involved in this invention can form a dense nano-armor layer on the bubble surface, inhibiting CO2 diffusion and improving foam stability. The nano-armor layer has strong interfacial viscoelasticity, effectively inhibiting CO2 cross-flow and controlling CO2 mobility, thus helping to expand the CO2 sequestration range and increase geological sequestration capacity.
[0007] The "two-dimensional nanomaterials" mentioned in this invention refer to nanomaterials with one dimension at the nanoscale, such as nanosheets and nanofilms.
[0008] This invention first provides a method for preparing organic Janus nanosheets, comprising the following steps:
[0009] S1. The hydrophobic end molecules containing long-chain alkanes and primary amino groups are thoroughly ground and then slowly stirred in a mixture of ethanol or other monohydric alcohols and water at a temperature 3-5°C above room temperature until the solution is clear and the hydrophobic end molecules are completely dissolved. During this process, large-scale shaking should be avoided to allow them to spontaneously arrange themselves in an orderly manner.
[0010] S2. Add the hydrophilic end molecule containing hydroxyl and hydrophilic groups to the solution in step S1, add a small amount of weak acid and adjust the pH to 6.0-6.5, and gradually lower the temperature by 5-10°C every 20-30 minutes under an inert atmosphere until it reaches room temperature to synthesize the organic Janus nanosheet monomer. During this process, a significant color deepening will be observed, indicating that a nucleophilic addition reaction has occurred.
[0011] S3. Add ethanol to the solution from step S2 to adjust the solvent composition ratio, and add a weak acid dropwise to adjust the pH to 6.0-6.5. Let the reaction stand for 5-10 minutes. Then adjust the pH to 7.0-8.0, add sodium ethoxide, adjust the temperature to 70-85°C, add a reflux condenser and carry out the reaction under an inert atmosphere. Add NaOH to the system to adjust the pH to 8.0-9.0, stir until completely dissolved, stop stirring and let stand to obtain the organic Janus nanosheets.
[0012] In the above preparation method, the hydrophobic end molecule is a long-chain alkane containing a primary amine group, such as octadecylamine or dodecylamine;
[0013] The hydrophilic end molecule is an aromatic hydrocarbon compound containing phenolic hydroxyl groups and hydrophilic groups, such as dopamine, tyramine, or 2,4-dihydroxyphenylethylamine.
[0014] In the above preparation method, in step S1, the mass ratio of the hydrophobic end molecule, the ethanol and the water is 1:20-100:10-50.
[0015] In the above preparation method, step S1, the spontaneous ordered arrangement step is as follows:
[0016] The hydrophobic end molecules are added to the ethanol or other monohydric alcohol solution and refluxed at 60–80°C until dissolved; then water is added until there is no turbidity and stirring is stopped; the spontaneous ordered arrangement is carried out at 50–70°C.
[0017] In the above preparation method, the reflux conditions in step S2 are as follows:
[0018] The initial temperature is 50-80℃, and the temperature is reduced by 5-10℃ every 20-30 minutes until it reaches room temperature.
[0019] In the system of step S2, the mass percentage of the hydrophilic end molecules is 0.5% to 1.5%.
[0020] The mass ratio of the hydrophilic end molecules to the hydrophobic end molecules is 1:2 to 5, preferably 1:3.
[0021] In the above preparation method, in step S3, the reaction time is 4 to 8 hours;
[0022] The mass ratio of ethanol to the solution obtained in step S2 is 1:1.5 to 3;
[0023] In the system of step S3, the mass percentage of sodium ethoxide is 0.1-0.4%.
[0024] In the above preparation method, step S3, after the reaction is completed, further includes the following purification step:
[0025] Ethanol and water were added sequentially to the system in step S3 for ultrasonic dispersion and centrifugation to obtain a solid product. The organic Janus nanosheets were then freeze-dried under vacuum and stored as powder. The thickness of the obtained Janus nanosheets was controlled between 5 and 40 nm.
[0026] The above ultrasonic dispersion step can be performed in small batches.
[0027] The ultrasonic dispersion time using the ethanol is 20–60 min;
[0028] The ultrasonic dispersion time using the water is 20–60 min;
[0029] The above ultrasonic dispersion step can be repeated 2 to 5 times.
[0030] Step S3 yields a solution in which the volume ratio of ethanol to water is 1:4 to 10:8 to 20.
[0031] The two-dimensional organic Janus nanosheets prepared by the method of this invention are synthesized by hydrophobic and hydrophilic end groups in proportion, resulting in a more uniform distribution of groups and stronger Janus properties; the aspect ratio of the Janus nanosheets can be controlled, and the shape is regular.
[0032] The two-dimensional organic Janus nanosheets prepared by the method of this invention were subjected to contact angle tests, which showed that they have the ability to reverse wettability.
[0033] Based on the two-dimensional organic Janus nanosheets, the present invention further provides a stable water-based CO2 foam, which is made of CO2 and a liquid phase;
[0034] The liquid phase is an aqueous solution of the surfactant and the organic Janus nanosheets;
[0035] The water-based CO2 foam has a foam mass of 40% to 95%, more preferably 60% to 90%.
[0036] Specifically, in the liquid phase, the mass percentage of the surfactant is less than 1.0%, preferably 0.2% to 1.0%;
[0037] The organic Janus nanosheets have a mass percentage of less than 0.7%, preferably 0.05% to 0.7%, more preferably 0.05%, 0.08%, 0.1%, 0.15%, 0.18%, 0.2%, 0.3%, 0.4%, or a range of any two of the above values;
[0038] The surfactant can be anionic, cationic, or nonionic surfactant. The anionic surfactant is preferably sodium dodecyl sulfate (SDS), the cationic surfactant is preferably hexadecyltrimethylammonium bromide (CTAB), and the nonionic surfactant is preferably octylphenyl polyoxyethylene ether (TX-100).
[0039] The method for preparing water-based CO2 foam according to the present invention includes the following steps:
[0040] Sa, add the organic Janus nanosheets to the aqueous solution of the surfactant and stir for 10-20 min to obtain a foam base liquid;
[0041] Sb. Inject CO2 into the foam base liquid and stir and foam using the Waring Blender method to obtain the water-based CO2 foam;
[0042] The stirring speed can be 7000-9000 rpm, and the stirring time can be 3-10 min.
[0043] The foaming and foam stabilization experiments were conducted on the organic Janus nanosheet ultra-stable water-based CO2 foam prepared by the method of the present invention. The results showed that the composite foam of nonionic surfactant and organic Janus nanosheet had the strongest stability, and the foam stability was even stronger with the increase of nanosheet concentration.
[0044] The present invention has the following beneficial effects:
[0045] (1) In the ultra-stable water-based CO2 foam system of the present invention, two-dimensional organic Janus nanosheets can form a dense nano-armor layer on the surface of the bubble, which inhibits CO2 diffusion. Due to the large aspect ratio of the sheets, they can form an efficient coating on the surface of the bubble. The organic Janus nanosheets can form a dense nano-armor layer at low concentrations to stabilize the CO2 foam, which helps to efficiently carry and seal CO2 in underground reservoirs.
[0046] (2) The ultra-stable water-based CO2 foam system of the present invention has strong viscoelasticity at the interface of the nano-armor layer and high flow resistance in porous media. Therefore, it can effectively block cross-flow channels, inhibit CO2 fingering, thereby controlling CO2 flow rate, expanding the CO2 storage range, and increasing the storage capacity.
[0047] (3) In the ultra-stable water-based CO2 foam system of the present invention, Janus nanosheets have electron-donating groups (carbonyl groups) and Lewis base properties due to the hydrophilic / hydrophobic group structure characteristics in the synthesis and preparation process, which makes them more compatible with CO2 molecules and have a better CO2 gas encapsulation effect, which helps to achieve the purpose of carbon capture, utilization and storage.
[0048] (4) In the ultra-stable water-based CO2 foam system of the present invention, the hydrophilic / hydrophobic groups do not participate in the reaction during the synthesis of two-dimensional organic Janus nanosheets. Therefore, they can be replaced with other similar groups to flexibly change the hydrophilic and hydrophobic groups of Janus nanosheets. The reactants react in proportion to ensure that the hydrophobic end groups and hydrophilic end groups are formed into sheets in a fixed ratio. Therefore, the amphiphilic groups are more evenly distributed and the prepared nanosheets have more significant Janus characteristics.
[0049] (5) In the ultra-stable water-based CO2 foam system of the present invention, the synthesis of two-dimensional organic Janus nanosheets does not require the construction of a phase interface. The preparation method is simple, the reaction conditions are mild, the synthesis process is short, the yield of Janus nanosheets is high, and the aspect ratio of the nanosheets can be controlled by adjusting the solution pH and the synthesis time to obtain Janus nanosheets within the target size range. Attached Figure Description
[0050] Figure 1 SEM image of the organic Janus nanosheets prepared in Example 1 of this invention.
[0051] Figure 2 The contact angles of the organic Janus nanosheets prepared in Example 1 of this invention before and after wetting modification on hydrophilic and hydrophobic surfaces are shown.
[0052] Figure 3 The image shows the particle size intensity of Janus nanosheets prepared under different pH values and reaction times in Example 2 of this invention.
[0053] Figure 4 The foaming volume and liquid half-life of the organic Janus nanosheets prepared in Example 3 of this invention, when combined with a nonionic surfactant, change with the concentration of Janus nanosheets. Detailed Implementation
[0054] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0055] Unless otherwise specified, all materials and reagents used in the following examples are commercially available.
[0056] Example 1: Synthesis of Organic Janus Nanosheets
[0057] (1) Hydrophobic end molecules are spontaneously ordered.
[0058] After thoroughly grinding 1.2g of octadecylamine (ODA), add it to 40g of ethanol solution. Stir and reflux in a 75℃ constant temperature water bath until the octadecylamine is completely dissolved. Slowly add 20g of deionized water to the solution. Stop stirring when the solution is clear, allowing the octadecylamine molecules to spontaneously and orderly arrange themselves in the ethanol-water system. Adjust the temperature of the water bath to 60-65℃.
[0059] (2) Synthesis of organic Janus nanosheet monomers
[0060] Take 0.4g of dopamine (DA) and add it to the solution in (1). Add acetic acid to adjust the pH to 6.0-6.5. Reflux under nitrogen atmosphere. Set the initial temperature to 60℃ and decrease it by 5℃ every 20 minutes. Stop heating after 2 hours of reaction and let the solution cool naturally to room temperature to complete the synthesis of organic Janus nanosheet monomer.
[0061] (3) Synthesis of organic Janus nanosheets
[0062] Add 40g of ethanol to the solution in (2), and add acetic acid to adjust the pH to 6.0-6.5. Heat the solution in a water bath and reflux for 7 minutes. Add ammonia to adjust the pH to 7.5. Add 0.2g of sodium ethoxide and adjust the temperature to 85℃. Stir at a constant temperature for 6 hours under nitrogen atmosphere. Add NaOH to adjust the pH to 8.0-9.0. Stop stirring after the solution is fully mixed and dissolved. Cool to room temperature and take out the solution with a thickness of 20-30nm.
[0063] (4) Purification of organic Janus nanosheets
[0064] Each time, take 20 mL of solution (3), mix thoroughly with 100 mL of ethanol solution, disperse ultrasonically and centrifuge for 20 minutes, remove the supernatant, retain the solid product, add 200 mL of deionized water to the separated product, disperse ultrasonically and centrifuge for 20 minutes, remove the supernatant, and retain the solid product. Repeat the above two steps 2-3 times to obtain organic Janus nanosheets. After vacuum freeze-drying, obtain powdered organic Janus nanosheets for storage.
[0065] Figure 1 The image shows a SEM image of the organic Janus nanosheets obtained in this embodiment. As can be seen, the organic Janus nanosheets prepared by this invention have a two-dimensional sheet structure.
[0066] Figure 2 The contact angles of the organic Janus nanosheets prepared in this embodiment before and after wetting modification on hydrophilic and hydrophobic surfaces demonstrate that the nanosheet material synthesized in this invention possesses amphiphilic properties.
[0067] The glass substrate exhibits hydrophilic properties with a water contact angle of 57.6°. After hydrophobic modification, the contact angle increases to 136.1°. Coating the nanosheets onto both substrates resulted in a wettability reversal, transforming the original hydrophilic / hydrophobic surface into a hydrophobic / hydrophilic surface. Therefore, the contact angle results confirm that the nanosheets possess amphiphilic properties.
[0068] Example 2: Controllable preparation of organic Janus nanosheets with different particle sizes
[0069] The operation steps are the same as in Example 1, except that the pH value of the ammonia solution in the synthesis of organic Janus nanosheets in step (3) is changed, and the total reaction time in steps (2) and (3) is changed to test the effect of different pH values and different reaction times on the particle size of Janus nanosheets.
[0070] Figure 3 The graphs show the particle size distribution of the nanosheets prepared under different pH values and reaction times. It can be seen that the particle size of Janus nanosheets decreases with increasing pH value and decreasing reaction time. The size of the Janus nanosheets can be controlled by adjusting the reaction time and pH value.
[0071] Example 3: Preparation of ultrastable water-based CO2 foam using organic Janus nanosheets
[0072] Prepare a TX-100 surfactant solution with a mass percentage of 0.4%, stir for 5 min, then dissolve the organic Janus nanosheets prepared in Example 1 in the surfactant solution and stir for 20 min to obtain a foam base liquid composed of Janus nanosheets and surfactant.
[0073] Pour the foam base liquid into a mixing cup, then seal the mixing cup and introduce CO2 to create a CO2 environment inside the cup. Use the Waring Blender method to stir and foam the foam base liquid at a stirring speed of 8000 rpm for 3 minutes to obtain CO2 foam. The foam quality can be controlled from 40% to 95%, and can be further controlled from 60% to 90%.
[0074] Figure 4 The foaming effect of compounding 0.4% nonionic surfactant with different mass percentages of Janus nanosheets can be observed as follows:
[0075] As the mass percentage of Janus nanosheets gradually increases to 0.15%, the nanosheet material in the solution is continuously adsorbed onto the surface of the bubbles. Utilizing its Janus properties and sheet-like morphology, it gradually forms an armor-like coating state to prevent bubble drainage and aggregation, thereby improving foam stability.
[0076] As the concentration of Janus nanosheets increases further, due to the limited interfacial area on the bubble surface, the nanosheets continuously aggregate and stack until larger bubbles can no longer withstand the adsorption of a large number of nanosheets and rupture. The nanosheets return to the liquid phase, causing a sharp increase in solution viscosity. However, this increase in solution viscosity significantly reduces the precipitation rate of smaller bubbles in the system. Therefore, during this stage, the foam volume of the foam system decreases, and the precipitation half-life gradually increases.
Claims
1. A method for preparing organic Janus nanosheets, comprising the following steps: S1. The hydrophobic end molecules are spontaneously ordered in a mixture of ethanol and water; S2. Add the hydrophilic end molecules to the solution in step S1, adjust the pH to 6.0-6.5, and reflux under an inert atmosphere to synthesize the organic Janus nanosheet monomer. S3. Add ethanol to the solution from step S2 and adjust the pH to 6.0–6.5, then heat under reflux; then adjust the pH to 7.0–8.0, add sodium ethoxide, adjust the temperature to 70–85°C, and react under an inert atmosphere. Add NaOH to adjust the pH to 8.0–9.0, and stir until completely dissolved to obtain the organic Janus nanosheets.
2. The preparation method according to claim 1, characterized in that: The hydrophobic end molecule is octadecylamine or dodecylamine; The hydrophilic end molecule is dopamine, tyramine, or 2,4-dihydroxyphenylethylamine.
3. The preparation method according to claim 1 or 2, characterized in that: In step S1, the mass ratio of the hydrophobic end molecule, the ethanol and the water is 1:20-100:10-50.
4. The preparation method according to any one of claims 1-3, characterized in that: In step S1, the steps for the spontaneous ordered arrangement are as follows: The hydrophobic end molecules are added to the ethanol and refluxed at 60–80°C until dissolved; then the water is added until there is no turbidity and stirring is stopped; the spontaneous ordered arrangement is carried out at 50–70°C.
5. The preparation method according to any one of claims 1-4, characterized in that: In step S2, the conditions for reflux are as follows: The initial temperature is 50-80℃, and the temperature is reduced by 5-10℃ every 20-30 minutes until it reaches room temperature. In the system of step S2, the mass percentage of the hydrophilic end molecules is 0.5% to 1.5%. The mass ratio of the hydrophilic end molecule to the hydrophobic end molecule is 1:2 to 5.
6. The preparation method according to any one of claims 1-5, characterized in that: In step S3, the reaction time is 4 to 8 hours; The mass ratio of ethanol to the solution obtained in step S2 is 1:1.5 to 3; In the system of step S3, the mass percentage of sodium ethoxide is 0.1-0.4%.
7. The preparation method according to any one of claims 1-6, characterized in that: In step S3, after the reaction is completed, the following purification step is also included: Ethanol and water were added sequentially to the system in step S3 for ultrasonic dispersion and centrifugation to obtain a solid product. Step S3 yields a solution in which the volume ratio of ethanol to water is 1:4 to 10:8 to 20.
8. Organic Janus nanosheets prepared by the method according to any one of claims 1-7; The Janus nanosheets have a thickness of 5–40 nm.
9. The application of the organic Janus nanosheets of claim 8 in carbon utilization and storage; The organic Janus nanosheets are used to form water-based CO2 foam.
10. An organic Janus nanosheet ultra-stable water-based CO2 foam, made from CO2 and a liquid phase; The liquid phase is an aqueous solution of a surfactant and the organic Janus nanosheets of claim 8; The water-based CO2 foam has a foam mass of 40% to 95%.
11. The water-based CO2 foam according to claim 10, characterized in that: In the liquid phase, the mass percentage of the surfactant is less than 1.0%; The organic Janus nanosheets contain less than 0.7% of the total amount. The surfactant is an anionic surfactant, a cationic surfactant, or a nonionic surfactant.
12. The method for preparing the water-based CO2 foam according to claim 10 or 11, comprising the following steps: Sa, add the organic Janus nanosheets to the aqueous solution of the surfactant and stir to obtain a foam base liquid; Sb. Inject CO2 into the foam base liquid and stir and foam using the Waring Blender method to obtain the water-based CO2 foam.
13. The application of the water-based CO2 foam of claim 10 or 11 in CO2 geological sequestration and foam flooding.