A functionalized EVA material and its application
By adding specific resins and polymers to the EVA material, the bonding and oxidation resistance of the EVA functional layer are improved, and the problems of insufficient bonding and poor oxidation resistance in the prior art are solved, thereby achieving high transparency and barrier properties Good paper-plastic composite film.
Patent Information
- Application Number
- CN202310541085.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-15
AI Technical Summary
The adhesion between the existing EVA functional layer and the base layer and paper is not strong, the oxidation resistance is poor, and it is easy to discolor, which affects the performance of the paper-plastic composite film.
Add terpene resin, branched polyethylene and polypropylene carbonate to the ethylene-vinyl acetate copolymer to produce a functionalized EVA material, which improves adhesion, oxidation resistance and transparency, and blends and The functional layer is formed by coating and a pre-coated film is prepared in combination with the base layer.
It realizes strong bonding with the base paper, oxidation resistance, high transparency, good barrier properties, and is not prone to yellowing, and improves the overall performance and service life of the paper-plastic composite film.
Smart Images

Figure BDA0004227952320000041 
Figure BDA0004227952320000042 
Figure BDA0004227952320000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional composite membranes, and in particular relates to a functionalized EVA material and application thereof. Background Art
[0002] Paper or printed paper can be laminated with plastic film to form a paper-plastic composite film. After lamination, a thin and transparent plastic film is added to the surface of the paper, making the surface smoother and brighter, greatly improving the gloss and fastness of the printed matter, extending the service life of the product, and playing a protective role in waterproofing, anti-fouling, wear resistance, folding resistance, chemical corrosion resistance, etc., and even some surface defects in the printing process can be compensated to a large extent.
[0003] Paper or printed paper is usually compounded with a functional layer of a pre-coated film to obtain a paper-plastic composite film. The pre-coated film usually includes a base layer and a functional layer. The base layer is generally made of a biaxially oriented polypropylene film (BOPP) or a biaxially oriented polyester film (PET), and the functional layer is generally made of EVA (ethylene-vinyl acetate copolymer). However, the existing functional layer made of EVA (ethylene-vinyl acetate copolymer) has weak adhesion to the base layer and paper, and the functional layer has poor oxidation resistance, and the pre-coated film is prone to discoloration. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a functionalized EVA material. By adding terpene resin, branched polyethylene and polypropylene carbonate with specific structure or performance to ethylene-vinyl acetate copolymer, a functionalized EVA material with strong composite bonding with base paper, oxidation resistance, high transparency, high barrier and not easy to yellow is prepared.
[0005] In a first aspect of the present invention, a functionalized EVA material is provided, comprising the following raw materials by weight: 50-65% ethylene-vinyl acetate copolymer, 10-20% terpene resin, 7-12% branched polyethylene, and 8-15% polypropylene carbonate;
[0006] The terpene resin has a softening point of 60 to 100° C. and an acid value of 70 to 110 mgKOH / g;
[0007] The branched polyethylene has a weight average molecular weight of 100,000 to 350,000 g / mol, a degree of branching of 80 to 120, a methyl branch content of 52 to 61.2%, an ethyl branch content of 9.5 to 16.2%, and a propyl branch content and a branch content of 4 or more carbon atoms of 22.6 to 38.5%;
[0008] The number average molecular weight of the polypropylene carbonate is 3,000 to 30,000 g / mol, the elongation at break is 800 to 1000%, and the melt index at 170° C. and 2.16 kg is 20 to 30 g / 10 min.
[0009] Preferably, the functionalized EVA material comprises the following raw materials by weight: 60% ethylene-vinyl acetate copolymer, 17% terpene resin, 10% branched polyethylene, and 8% polypropylene carbonate.
[0010] Preferably, the terpene resin has a softening point of 60 to 80° C. and an acid value of 70 to 85 mgKOH / g.
[0011] Preferably, the terpene resin has a softening point of 80 to 100° C. and an acid value of 90 to 110 mgKOH / g.
[0012] Preferably, the weight average molecular weight of the branched polyethylene is 100,000 to 180,000 g / mol, the degree of branching is 110 to 120, the methyl branch content is 52 to 56%, the ethyl branch content is 13 to 16.2%, and the propyl branch content and the branch content containing more than 4 carbon atoms are 27.8 to 35%.
[0013] Preferably, the weight average molecular weight of the branched polyethylene is 300,000 to 350,000 g / mol, the degree of branching is 80 to 105, the methyl branch content is 57 to 61.2%, the ethyl branch content is 9.5 to 12.7%, and the propyl branch content and the branch content containing more than 4 carbon atoms are 22.6 to 30.5%.
[0014] Preferably, the polypropylene carbonate has a number average molecular weight of 3,000 to 10,000 g / mol, an elongation at break of 920 to 1000%, and a melt index of 25 to 30 g / 10 min at 170° C. and 2.16 kg.
[0015] Preferably, the polypropylene carbonate has a number average molecular weight of 20,000 to 30,000 g / mol, an elongation at break of 800 to 900%, and a melt index of 20 to 24 g / 10 min at 170° C. and 2.16 kg.
[0016] Preferably, the functionalized EVA material further comprises 3-8% of a compatibilizer, and the compatibilizer is selected from polyvinyl acetate with a degree of polymerization of 600-900.
[0017] More preferably, the functionalized EVA material further comprises 5% of a compatibilizer, and the compatibilizer is selected from polyvinyl acetate with a degree of polymerization of 800.
[0018] In a second aspect of the present invention, a pre-coating film is provided, comprising a base layer and a functional layer, wherein the functional layer is composed of the functionalized EVA material, and the functional layer is disposed on the base layer.
[0019] Preferably, the thickness of the functional layer is 6-10 μm.
[0020] More preferably, the thickness of the functional layer is 8 μm.
[0021] Preferably, the base layer includes at least one of a biaxially stretched polyester layer, a biaxially stretched nylon layer, and a biaxially stretched polypropylene layer.
[0022] Preferably, the thickness of the base layer is 10-20 μm.
[0023] More preferably, the thickness of the base layer is 15 μm.
[0024] In a third aspect of the present invention, a method for preparing the pre-coating film is provided, comprising the following steps:
[0025] S1. The ethylene-vinyl acetate copolymer, the terpene resin, the branched polyethylene, the polypropylene carbonate and the optional compatibilizer are melt blended to obtain a functionalized EVA material;
[0026] S2. Coating or co-extrude the functionalized EVA material onto the base layer to obtain a functional film. DETAILED DESCRIPTION
[0027] In order to enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0028] The color number of terpene resin is 0-1.
[0029] The terpene resin raw material is selected from the following table:
[0030] Terpene resin number Softening point(℃) Acid value (mgKOH / g) TR-1 60 70 TR-2 80 85 TR-3 80 90 TR-4 100 110 TR-5 50 60 TR-6 110 120
[0031] The branched polyethylene raw material is selected from the following table:
[0032]
[0033] The polypropylene carbonate raw material is selected from the following table:
[0034]
[0035] Example 1: Preparation of pre-coating film.
[0036] S1. By weight content, 60% ethylene-vinyl acetate copolymer, 17% terpene resin TR-1, 10% branched polyethylene PE-1, 8% polypropylene carbonate PPC-1 and 5% polyvinyl acetate with a degree of polymerization of 600 were melt blended to obtain a functionalized EVA material;
[0037] S2. The functionalized EVA material is coated on the 15 μm biaxially oriented polyester layer, and pressed to form an 8 μm functional layer on the 15 μm biaxially oriented polyester layer to obtain a 23 μm pre-coated film.
[0038] Example 2: Preparation of pre-coating film.
[0039] S1. By weight content, 60% ethylene-vinyl acetate copolymer, 17% terpene resin TR-2, 10% branched polyethylene PE-2, 8% polypropylene carbonate PPC-2 and 5% polyvinyl acetate having a degree of polymerization of 900 were melt blended to obtain a functionalized EVA material;
[0040] S2. The functionalized EVA material is coated on the 15 μm biaxially oriented polyester layer, and pressed to form an 8 μm functional layer on the 15 μm biaxially oriented polyester layer to obtain a 23 μm pre-coated film.
[0041] Example 3: Preparation of pre-coating film.
[0042] The branched polyethylene PE-1 in Example 1 was replaced by branched polyethylene PE-3, and the remaining steps were the same as in Example 1.
[0043] Example 4: Preparation of pre-coating film.
[0044] The branched polyethylene PE-1 in Example 1 was replaced by branched polyethylene PE-4, and the remaining steps were the same as in Example 1.
[0045] Example 5: Preparation of pre-coating film.
[0046] The polypropylene carbonate PPC-1 in Example 1 was replaced by polypropylene carbonate PPC-3, and the remaining steps were the same as in Example 1.
[0047] Example 6: Preparation of pre-coating film.
[0048] The polypropylene carbonate PPC-1 in Example 1 was replaced by polypropylene carbonate PPC-4, and the remaining steps were the same as in Example 1.
[0049] Example 7: Preparation of pre-coating film.
[0050] S1. By weight content, 60% ethylene-vinyl acetate copolymer, 17% terpene resin TR-3, 10% branched polyethylene PE-1, 8% polypropylene carbonate PPC-1 and 5% polyvinyl acetate with a degree of polymerization of 600 were blended and melted to obtain a functionalized EVA material;
[0051] S2. The functionalized EVA material is coated on the 15 μm biaxially oriented polyester layer, and pressed to form an 8 μm functional layer on the 15 μm biaxially oriented polyester layer to obtain a 23 μm pre-coated film.
[0052] Example 8: Preparation of pre-coating film.
[0053] The terpene resin TR-3 in Example 7 was replaced by the terpene resin TR-4, and the remaining steps were the same as in Example 7.
[0054] Comparative Example 1: Preparation of pre-coating film.
[0055] The terpene resin TR-1 in Example 1 was replaced with a rosin resin having the same softening point and acid value, and the remaining steps were the same as in Example 1.
[0056] Comparative Example 2: Preparation of pre-coating film.
[0057] The terpene resin TR-3 in Example 7 was replaced with a rosin resin having the same softening point and acid value, and the remaining steps were the same as in Example 7.
[0058] Comparative Example 3: Preparation of pre-coating film.
[0059] The terpene resin TR-1 in Example 1 was replaced by the terpene resin TR-5, and the remaining steps were the same as in Example 1.
[0060] Comparative Example 4: Preparation of pre-coating film.
[0061] The terpene resin TR-1 in Example 1 was replaced by terpene resin TR-6, and the remaining steps were the same as in Example 1.
[0062] Comparative Example 5: Preparation of pre-coating film.
[0063] The branched polyethylene PE-1 in Example 1 was replaced by branched polyethylene PE-5, and the remaining steps were the same as in Example 1.
[0064] Comparative Example 6: Preparation of pre-coating film.
[0065] The branched polyethylene PE-1 in Example 1 was replaced by branched polyethylene PE-6, and the remaining steps were the same as in Example 1.
[0066] Comparative Example 7: Preparation of pre-coating film.
[0067] The polypropylene carbonate PPC-1 in Example 1 was replaced by polypropylene carbonate PPC-5, and the remaining steps were the same as in Example 1.
[0068] Comparative Example 8: Preparation of pre-coating film.
[0069] The polypropylene carbonate PPC-1 in Example 1 was replaced by polypropylene carbonate PPC-6, and the remaining steps were the same as in Example 1.
[0070] Comparative Example 9: Preparation of pre-coating film.
[0071] The 60% ethylene-vinyl acetate copolymer, 17% terpene resin TR-1, 10% branched polyethylene PE-1, 8% polypropylene carbonate PPC-1 and 5% polyvinyl acetate with a degree of polymerization of 600 in Example 1 were melt-blended and replaced with 62% ethylene-vinyl acetate copolymer, 18% terpene resin TR-1, 11% branched polyethylene PE-1 and 9% polypropylene carbonate PPC-1, and the other steps remained unchanged.
[0072] Comparative Example 10: Preparation of pre-coating film.
[0073] The polyvinyl acetate with a degree of polymerization of 600 in Example 1 is replaced by polyvinyl acetate with a degree of polymerization of 400, and the remaining steps are the same as in Example 1.
[0074] Comparative Example 11: Preparation of pre-coating film.
[0075] The polyvinyl acetate with a degree of polymerization of 600 in Example 1 is replaced by polyvinyl acetate with a degree of polymerization of 1200, and the remaining steps are the same as in Example 1.
[0076] Performance test: The pre-coated films of Examples 1 to 8 and Comparative Examples 1 to 11 were respectively compounded with coated paper by thermal bonding to obtain paper-plastic composite films of Examples 9 to 16 and Comparative Examples 12 to 22, and performance tests were performed. The test results are shown in Table 1.
[0077] Adhesion test: refer to the standard GB8808-1988 test method.
[0078] Yellowing resistance test: The test was conducted in a UV-340 fluorescent UV aging test chamber at a temperature of 50°C and an irradiation intensity of 0.68W / m 2 The irradiation time was 168 h, and ΔE was tested using a colorimeter.
[0079] Shrinkage test: Test in accordance with GB / T 13542.2-2009.
[0080] Water permeability: Tested in accordance with GB / T 1037-2021.
[0081] Haze: Tested using a standard haze meter.
[0082] Table 1. Test results of paper-plastic composite film properties.
[0083]
[0084] As can be seen from Table 1, the paper-plastic composite films of Examples 9-16 prepared from the functionalized EVA materials of Examples 1-8 have good adhesion, heat resistance and yellowing resistance, use less glue layer material, achieve better viscosity, and can achieve lightweight; compared with other examples and comparative examples, the paper-plastic composite films of Examples 11 and 12 have better yellowing resistance; the paper-plastic composite films of Examples 13 and 14 have better barrier properties; the paper-plastic composite films of Examples 15 and 16 have better transparency; polypropylene carbonate has the problem of poor thermal stability, and the addition of polyvinyl acetate can improve the thermal stability of polypropylene carbonate, thereby improving the thermal stability of the paper-plastic composite film, comparative example 20 does not contain polyvinyl acetate in the functionalized EVA material, the thermal stability of the paper-plastic composite film is greatly reduced, and the thermal shrinkage rate is greatly improved, the polymerization degree of polyvinyl acetate in comparative example 21 decreases and the polymerization degree of polyvinyl acetate in comparative example 22 increases, the thermal stability of the prepared paper-plastic composite film is slightly reduced, and the thermal shrinkage rate is slightly improved.
[0085] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that after reading the specification of this application, the technicians can still modify or replace the specific implementation mode of the present invention with equivalents, but these modifications or changes do not deviate from the scope of protection of the pending claims of the present application.
Claims
1. A functionalized EVA material, characterized in that: The method is composed of the following raw materials by weight: 50-65% of ethylene-vinyl acetate copolymer, 10-20% of terpene resin, 7-12% of branched polyethylene, 8-15% of polypropylene carbonate and 3-8% of a compatibilizer; The compatibilizer is selected from polyvinyl acetate with a degree of polymerization of 600 to 900; The terpene resin has a softening point of 60-100° C. and an acid value of 70-110 mgKOH / g; The branched polyethylene has a weight average molecular weight of 100,000 to 350,000 g / mol, a degree of branching of 80 to 120, a methyl branch content of 52 to 61.2%, an ethyl branch content of 9.5 to 16.2%, and a propyl branch content and a branch content of 4 or more carbon atoms of 22.6 to 38.5%; The number average molecular weight of the polypropylene carbonate is 3,000 to 30,000 g / mol, the elongation at break is 800 to 1000%, and the melt index at 170° C. and 2.16 kg is 20 to 30 g / 10 min.
2. The functionalized EVA material according to claim 1, characterized in that The terpene resin has a softening point of 60-80° C. and an acid value of 70-85 mgKOH / g.
3. The functionalized EVA material according to claim 1, characterized in that The terpene resin has a softening point of 80-100° C. and an acid value of 90-110 mgKOH / g.
4. The functionalized EVA material according to claim 1, characterized in that The branched polyethylene has a weight average molecular weight of 100,000 to 180,000 g / mol, a degree of branching of 110 to 120, a methyl branch content of 52 to 56%, an ethyl branch content of 13 to 16.2%, and a propyl branch content and a branch content of more than 4 carbon atoms of 27.8 to 35%.
5. The functionalized EVA material according to claim 1, characterized in that The weight average molecular weight of the branched polyethylene is 300,000-350,000 g / mol, the degree of branching is 80-105, the content of methyl branches is 57-61.2%, the content of ethyl branches is 9.5-12.7%, and the content of propyl branches and branches containing more than 4 carbon atoms is 29.3-30.5%.
6. The functionalized EVA material according to claim 1, characterized in that The number average molecular weight of the polypropylene carbonate is 3,000 to 10,000 g / mol, the elongation at break is 920 to 1000%, and the melt index at 170° C. and 2.16 kg is 25 to 30 g / 10 min.
7. The functionalized EVA material according to claim 1, characterized in that The polypropylene carbonate has a number average molecular weight of 20,000 to 30,000 g / mol, an elongation at break of 800 to 900%, and a melt index of 20 to 24 g / 10 min at 170° C. and 2.16 kg.
8. A pre-coating film, characterized in that: It comprises a base layer and a functional layer, wherein the functional layer is composed of the functionalized EVA material according to any one of claims 1 to 7, and the functional layer is arranged on the base layer.
9. A method for preparing a pre-coating film as claimed in claim 8, characterized in that: The steps include: S1. The ethylene-vinyl acetate copolymer, the terpene resin, the branched polyethylene, the polypropylene carbonate and the compatibilizer are melt blended to obtain a functionalized EVA material; S2. coating or co-extruding the functionalized EVA material on the base layer to obtain a pre-coated film.
Citation Information
Patent Citations
Viscosity-increasing precoating film of biaxial tension
CN101402269A
BOPP (Biaxially-oriented Polypropylene) pre-coating basement membrane
CN102504716A
Digital pre-coating film and preparation method thereof
CN109337598A
Polypropylene composition and preparation method thereof
CN111253682A
Co-extrusion type instant composite paper BOPP film and preparation method thereof
CN111645388A