A modified and reused material for medical infusion bag and a preparation method thereof
By combining medical infusion bags with maleic anhydride, polyolefin elastomer, glass fiber and organic phosphorus modified nanosilica and other materials, a modified and reusable infusion bag with good mechanical and flame retardant properties was prepared, and the solution was solved The problem of waste of medical infusion bag resources has achieved efficient reuse.
Patent Information
- Application Number
- CN202310384871.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-04-12
AI Technical Summary
As a disposable medical equipment, medical infusion bags are directly treated as medical waste after being contaminated by the patient's blood, body fluids, or excrement, resulting in increased costs and waste of resources.
Using medical infusion bags to modify and reuse materials, the cleaned and dried infusion bags are grafted with maleic anhydride, and modified with polyolefin elastomer, glass fiber, organic phosphorus nanosilica and melamine cyanuric acid Combining materials such as salt, they are made of materials with good mechanical and flame retardant properties through twin screw extrusion and granulation.
It effectively improves the mechanical properties and flame retardant properties of the materials, solves the problem of insufficient mechanical properties caused by the mixed components during recycling and reuse of medical infusion bags, and realizes efficient reuse of resources.
Smart Images

Figure CN116376161B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of medical waste recycling and reuse, and in particular to a modified and reused material for a medical infusion bag and a preparation method thereof. Background Art
[0002] With the improvement of my country's overall national economic level and the development of medical science, more and more disposable medical devices are used in hospitals. They are widely used in the diagnosis and treatment of clinical medical care, effectively preventing and controlling hospital infections and improving work efficiency and medical care quality.
[0003] Medical infusion bags are disposable medical equipment that are not contaminated by the patient's blood, body fluids, or excrement. Directly treating them as medical waste increases costs and causes a waste of resources. Summary of the invention
[0004] Purpose of the invention: In view of the above technical problems, the present invention proposes a modified and reused material for medical infusion bags and a preparation method thereof.
[0005] The technical solutions adopted are as follows:
[0006] A modified and recycled material for a medical infusion bag, comprising, by weight:
[0007] PP resin 80-100 parts (PP: polypropylene resin);
[0008] 30-40 parts of recycled and modified resin from medical infusion bags;
[0009] POE-g-(GMA-co-MAH) 20-40 parts;
[0010] (POE: polyolefin elastomer, GMA: glycidyl methacrylate, MAH: maleic anhydride)
[0011] Glass fiber 10-40 parts;
[0012] 10-30 parts of organophosphorus modified nano silicon dioxide;
[0013] 1-3 parts of melamine cyanurate;
[0014] Additives 0-5 parts.
[0015] Further, in parts by weight, comprising:
[0016] PP resin 90 parts
[0017] 35 parts of recycled and modified resin for medical infusion bags;
[0018] POE-g-(GMA-co-MAH) 20 parts;
[0019] Glass fiber 20 parts;
[0020] 20 parts of organophosphorus modified nano-silicon dioxide;
[0021] 2 parts of melamine cyanurate;
[0022] 3 parts of additives.
[0023] Furthermore, the medical infusion bag is obtained by grafting and modifying the PP material of the recycled and modified resin with maleic anhydride after washing, drying, and crushing.
[0024] Furthermore, the preparation method of the medical infusion bag recycled and modified resin is as follows:
[0025] The medical infusion bag made of PP material is washed, dried, crushed, and added to acetone, and then maleic anhydride and peroxide initiator are added. After stirring evenly, the mixture is heated to completely volatilize the acetone, and the obtained material is added to a twin-screw extruder for extrusion and granulation.
[0026] Further, the preparation method of the POE-g-(GMA-co-MAH) is as follows:
[0027] POE, GMA, MAH and peroxide initiator are mixed evenly and added into a twin-screw extruder for reaction extrusion granulation. The obtained pellets are refluxed in hot toluene until they are completely dissolved. The toluene solution is then poured into acetone for precipitation. After precipitation is complete, the precipitate is filtered out and finally washed with acetone and dried.
[0028] Furthermore, the organophosphorus-modified nano-silica is obtained by bridging the organophosphorus with the nano-silica via a silane coupling agent KH560.
[0029] Furthermore, the organic phosphorus is DOPO or a DOPO derivative (DOPO: 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide).
[0030] Furthermore, the preparation method of the organophosphorus modified nano-silicon dioxide is as follows:
[0031] After the organophosphorus flame retardant and the silane coupling agent KH560 are uniformly mixed, they are heated to 140-160°C under the protection of inert gas and reacted for 6-10 hours to obtain an intermediate. Then, the intermediate and nano-silica are added to an ethanol / water solution and heated to 50-60°C and reacted for 12-24 hours.
[0032] Furthermore, the auxiliary agents include antioxidant 1010, antioxidant 168, and polyethylene wax.
[0033] The present invention also provides a method for preparing a modified and reused material for a medical infusion bag:
[0034] PP resin, medical infusion bag recycled modified resin, POE-g-(GMA-co-MAH), glass fiber, organophosphorus modified nano-silica, melamine cyanurate and additives are mixed evenly and then placed in a twin-screw extruder for extrusion granulation.
[0035] Beneficial effects of the present invention:
[0036] Medical infusion bags are directly crushed and reused as recycled materials, which will cause the mechanical properties of the materials to fail to meet the use requirements due to the mixed components. However, after being modified with MAH, the bonding performance with the new PP resin material is improved, and the blending has little effect on the mechanical properties. POE-g-(GMA-co-MAH) is obtained by reactive extrusion grafting highly reactive GMA and MAH on a POE elastomer as a matrix. As a toughening agent and compatibilizer, it can effectively improve the mechanical properties of the material. Nano-silicon dioxide has many special properties, such as surface size effect, volume effect, quantum effect, etc. Due to its poor compatibility with the PP resin matrix, its compatibility is improved after being modified with organic phosphorus, and it forms an NP-Si composite flame retardant system with melamine cyanurate to improve the flame retardant effect. After testing, the material prepared by recycling and reusing the medical infusion bags in the present invention has good mechanical properties and flame retardant properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a SEM cross-sectional morphology of the material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0038] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The technologies not mentioned in the present invention are all referenced to the prior art.
[0039] Embodiment 1:
[0040] A modified and recycled material for a medical infusion bag, comprising, by weight:
[0041] PP resin 90 parts
[0042] 35 parts of recycled and modified resin for medical infusion bags;
[0043] POE-g-(GMA-co-MAH) 20 parts;
[0044] Glass fiber 20 parts;
[0045] DOPO modified nano-silica 20 parts;
[0046] 2 parts of melamine cyanurate;
[0047] Antioxidant 1010 0.5 parts;
[0048] Antioxidant 168 0.5 parts;
[0049] 2 parts of polyethylene wax.
[0050] Among them, the preparation method of the recycled and modified resin for medical infusion bags is as follows:
[0051] 500g of PP medical infusion bag was washed, dried, and crushed and added to 1500mL of acetone. Then, 50g of maleic anhydride and 4g of dibenzoyl peroxide were added. After stirring evenly, the mixture was heated to completely volatilize the acetone. The resulting material was added to a twin-screw extruder for extrusion granulation. The screw speed of the twin-screw extruder was 140-150r / min, and the extrusion section temperature was 190-195°C.
[0052] The preparation method of POE-g-(GMA-co-MAH) is as follows:
[0053] 100g POE, 5g GMA, 4.3g MAH and 0.15g dibenzoyl peroxide initiator were mixed evenly and added into a twin-screw extruder for reaction extrusion granulation. The screw speed of the twin-screw extruder was 100-120r / min, and the temperature of the extrusion section was 180-200°C. The obtained pellets were refluxed in hot toluene until they were completely dissolved. The toluene solution was then poured into acetone for precipitation. After the precipitation was complete, the precipitate was filtered out and finally washed with acetone and dried.
[0054] The preparation method of DOPO-modified nano-silica is as follows:
[0055] Add 38g DOPO and 50g silane coupling agent KH560 into a reactor with a condenser and mix well. Heat to 150°C under nitrogen protection for 8h, distill off small molecules, then add the intermediate and 200g nano-silica into 1800mL ethanol / water solution (ethanol:water volume ratio is 5:1), heat to 60°C for 18h, filter, wash with ethanol and dry.
[0056] Preparation method of the above-mentioned modified and reused medical infusion bag material:
[0057] PP resin, medical infusion bag recycled modified resin, POE-g-(GMA-co-MAH), glass fiber, organophosphorus modified nano-silica, melamine cyanurate and additives are mixed evenly and placed in a twin-screw extruder for extrusion granulation. The screw speed of the twin-screw extruder is 200-220r / min, and the extrusion section temperature is 200-210℃.
[0058] Embodiment 2:
[0059] A modified and recycled material for a medical infusion bag, comprising, by weight:
[0060] PP resin 100 parts
[0061] 40 parts of recycled and modified resin for medical infusion bags;
[0062] POE-g-(GMA-co-MAH) 40 parts;
[0063] Glass fiber 40 parts;
[0064] 30 parts of DOPO modified nano-silica;
[0065] 3 parts of melamine cyanurate;
[0066] Antioxidant 1010 0.5 parts;
[0067] Antioxidant 168 0.5 parts;
[0068] 2 parts of polyethylene wax.
[0069] Preparation method of the above-mentioned modified and reused medical infusion bag material:
[0070] PP resin, medical infusion bag recycled modified resin, POE-g-(GMA-co-MAH), glass fiber, organophosphorus modified nano-silica, melamine cyanurate and additives are mixed evenly and placed in a twin-screw extruder for extrusion granulation. The screw speed of the twin-screw extruder is 200-220r / min, and the extrusion section temperature is 200-210℃.
[0071] The preparation method of the recycled and modified resin for medical infusion bags, POE-g-(GMA-co-MAH), and DOPO-modified nano-silica is the same as that in Example 1.
[0072] Embodiment 3:
[0073] A modified and recycled material for a medical infusion bag, comprising, by weight:
[0074] PP resin 80 parts
[0075] 30 parts of recycled and modified resin for medical infusion bags;
[0076] POE-g-(GMA-co-MAH) 20 parts;
[0077] Glass fiber 10 parts;
[0078] DOPO modified nano-silica 10 parts;
[0079] 1 part of melamine cyanurate;
[0080] Antioxidant 1010 0.5 parts;
[0081] Antioxidant 168 0.5 parts;
[0082] 2 parts of polyethylene wax.
[0083] Preparation method of the above-mentioned modified and reused medical infusion bag material:
[0084] PP resin, medical infusion bag recycled modified resin, POE-g-(GMA-co-MAH), glass fiber, organophosphorus modified nano-silica, melamine cyanurate and additives are mixed evenly and placed in a twin-screw extruder for extrusion granulation. The screw speed of the twin-screw extruder is 200-220r / min, and the extrusion section temperature is 200-210℃.
[0085] The preparation method of the recycled and modified resin for medical infusion bags, POE-g-(GMA-co-MAH), and DOPO-modified nano-silica is the same as that in Example 1.
[0086] Embodiment 4:
[0087] A modified and recycled material for a medical infusion bag, comprising, by weight:
[0088] PP resin 100 parts
[0089] 30 parts of recycled and modified resin for medical infusion bags;
[0090] POE-g-(GMA-co-MAH) 40 parts;
[0091] Glass fiber 10 parts;
[0092] 30 parts of DOPO modified nano-silica;
[0093] 1 part of melamine cyanurate;
[0094] Antioxidant 1010 0.5 parts;
[0095] Antioxidant 168 0.5 parts;
[0096] 2 parts of polyethylene wax.
[0097] Preparation method of the above-mentioned modified and reused medical infusion bag material:
[0098] PP resin, medical infusion bag recycled modified resin, POE-g-(GMA-co-MAH), glass fiber, organophosphorus modified nano-silica, melamine cyanurate and additives are mixed evenly and placed in a twin-screw extruder for extrusion granulation. The screw speed of the twin-screw extruder is 200-220r / min, and the extrusion section temperature is 200-210℃.
[0099] The preparation method of the recycled and modified resin for medical infusion bags, POE-g-(GMA-co-MAH), and DOPO-modified nano-silica is the same as that in Example 1.
[0100] Embodiment 5:
[0101] A modified and recycled material for a medical infusion bag, comprising, by weight:
[0102] PP resin 80 parts
[0103] 40 parts of recycled and modified resin for medical infusion bags;
[0104] POE-g-(GMA-co-MAH) 20 parts;
[0105] Glass fiber 40 parts;
[0106] DOPO modified nano-silica 10 parts;
[0107] 3 parts of melamine cyanurate;
[0108] Antioxidant 1010 0.5 parts;
[0109] Antioxidant 168 0.5 parts;
[0110] 2 parts of polyethylene wax.
[0111] Preparation method of the above-mentioned modified and reused medical infusion bag material:
[0112] PP resin, medical infusion bag recycled modified resin, POE-g-(GMA-co-MAH), glass fiber, organophosphorus modified nano-silica, melamine cyanurate and additives are mixed evenly and placed in a twin-screw extruder for extrusion granulation. The screw speed of the twin-screw extruder is 200-220r / min, and the extrusion section temperature is 200-210℃.
[0113] The preparation method of the recycled and modified resin for medical infusion bags, POE-g-(GMA-co-MAH), and DOPO-modified nano-silica is the same as that in Example 1.
[0114] Comparative Example 1:
[0115] It is basically the same as Example 1, except that the recycled resin of the medical infusion bag is not modified, that is, the medical infusion bag made of PP material is directly used as raw material after being cleaned, dried and crushed.
[0116] Comparative Example 2:
[0117] The method is substantially the same as Example 1, except that POE-g-(GMA-co-MAH) is not added.
[0118] Comparative Example 3:
[0119] The method is substantially the same as Example 1, except that POE-g-GMA is used instead of POE-g-(GMA-co-MAH).
[0120] Comparative Example 4:
[0121] It is basically the same as Example 1, except that the nano-silica is not modified by DOPO.
[0122] Performance Testing:
[0123] Prepare samples according to the methods in Examples 1-5 and Comparative Examples 1-4;
[0124] Impact strength is tested according to GB / T 1043.1-2008;
[0125] The bending strength is tested according to GB / T 9341-2000, and the indentation rate is 12mm / min;
[0126] Tensile performance: According to GB / T 1447-2005 test standard, tensile rate 10mm / min;
[0127] Limiting oxygen index (LOI) test is carried out according to ASTM D2863-2013;
[0128] There were 5 samples in each group, and the experimental results were averaged;
[0129] The test results are shown in Table 1 below:
[0130] Table 1:
[0131]
[0132] It can be seen from Table 1 above that the material prepared by recycling and reusing the medical infusion bag in the present invention has good mechanical properties and flame retardant properties.
[0133] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A modified and recycled material for medical infusion bags, characterized in that: In parts by weight, it includes: PP resin 80-100 parts; 30-40 parts of recycled and modified resin from medical infusion bags; POE-g-(GMA-co-MAH) 20-40 parts; Glass fiber 10-40 parts; 10-30 parts of organophosphorus modified nano silicon dioxide; 1-3 parts of melamine cyanurate; Additives 0-5 parts; The medical infusion bag recycled and modified resin is a medical infusion bag made of PP material, which is obtained by grafting and modifying with maleic anhydride after washing, drying and crushing; The preparation method of the POE-g-(GMA-co-MAH) is as follows: POE, GMA, MAH and peroxide initiator are mixed evenly and added into a twin-screw extruder for reaction extrusion granulation. The obtained pellets are refluxed in hot toluene until they are completely dissolved. The toluene solution is then poured into acetone for precipitation. After precipitation is complete, the precipitate is filtered to obtain the precipitate, and finally washed with acetone and dried. The organophosphorus modified nano-silica is obtained by bridging the organophosphorus with the nano-silica through the silane coupling agent KH560; The organophosphorus is DOPO; The preparation method of the organophosphorus modified nano silicon dioxide is as follows: After the organophosphorus flame retardant and the silane coupling agent KH560 are uniformly mixed, they are heated to 140-160°C under the protection of inert gas and reacted for 6-10 hours to obtain an intermediate. Then, the intermediate and nano-silica are added to an ethanol / water solution and heated to 50-60°C and reacted for 12-24 hours.
2. The modified and reused material for medical infusion bags according to claim 1, characterized in that: In parts by weight, it includes: PP resin 90 parts; 35 parts of recycled and modified resin for medical infusion bags; POE-g-(GMA-co-MAH) 20 parts; Glass fiber 20 parts; 20 parts of organophosphorus modified nano-silicon dioxide; 2 parts of melamine cyanurate; 3 parts of additives.
3. The modified and reused material for medical infusion bags according to claim 1, characterized in that: The preparation method of the medical infusion bag recycled and modified resin is as follows: The medical infusion bag made of PP material is washed, dried, crushed, and added to acetone, and then maleic anhydride and peroxide initiator are added. After stirring evenly, the mixture is heated to completely volatilize the acetone, and the obtained material is added to a twin-screw extruder for extrusion and granulation.
4. The modified and reused material for medical infusion bags according to claim 1, characterized in that: The auxiliary agents include antioxidant 1010, antioxidant 168 and polyethylene wax.
5. A method for preparing a modified and reused material for a medical infusion bag as claimed in any one of claims 1 to 4, characterized in that: PP resin, medical infusion bag recycled modified resin, POE-g-(GMA-co-MAH), glass fiber, organophosphorus modified nano-silica, melamine cyanurate and additives are mixed evenly and then placed in a twin-screw extruder for extrusion granulation.
Citation Information
Patent Citations
Toughened regenerated modified granule manufactured through polyolefin of waste medical plastic transfusion container
CN104140594A
Intelligent novel modified injection molding process for high-strength large garbage can
CN112659503A