A kind of sapphire substrate aluminum oxide polishing liquid and preparation method thereof

By optimizing the preparation of alumina powder by using macromolecular dispersants and polishing speed-accelerating agents, the problems of poor dispersion and low polishing efficiency of alumina polishing liquid are solved, and efficient polishing effects and low-cost production are achieved.

CN116376449BActive Publication Date: 2024-10-29HUANGPU INST OF MATERIALS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310207738.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-06
Publication Date
2024-10-29
Estimated Expiration
2043-03-06

AI Technical Summary

Technical Problem

Existing alumina polishing solutions have problems such as poor dispersion, low polishing efficiency, and excessive addition of chemical reagents when polishing sapphire substrates, resulting in poor polished product quality and low production efficiency.

Method used

Macromolecule dispersants are used to prepare the fine particle size of alumina powder, combined with polishing speed-increasing agents and pH regulators to form an alumina polishing liquid with good suspension properties, reduce the use of chemical reagents, and avoid the volatilization problem of hydrogen peroxide oxidant.

Benefits of technology

It improves the polishing rate and dispersion of alumina polishing fluid and reduces the risk of surface scratches. The surface roughness is less than 0.3nm, the removal rate reaches more than 15μm/h, and it is easy to store and produce on a large scale, with high cost performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116376449B_ABST
    Figure CN116376449B_ABST
Patent Text Reader

Abstract

The present invention discloses a sapphire substrate sheet alumina polishing liquid and a preparation method thereof. The sapphire substrate sheet alumina polishing liquid of the present invention is composed of alumina powder, a dispersant, a polishing accelerator, a pH regulator and water, wherein the dispersant is a macromolecular dispersant, and the particle size of the alumina powder is 0.5-1.0 μm. The sapphire substrate sheet alumina polishing liquid of the present invention is prepared by using a macromolecular dispersant and alumina powder with a fine particle size, has good suspension, less chemical reagent addition, high polishing efficiency and low cost. The preparation method of the sapphire substrate sheet alumina polishing liquid of the present invention can realize the large-scale production of the sapphire substrate sheet alumina polishing liquid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polishing liquid, and in particular to a sapphire substrate sheet aluminum oxide polishing liquid and a preparation method thereof. Background Art

[0002] Alumina polishing liquid is currently widely used in the polishing of sapphire substrates. However, there are many problems with the alumina polishing liquid on the market, such as poor dispersion of alumina, bottom compaction, precipitation, insufficient removal rate, scratches and edge collapse, which seriously affect the quality of the polished products.

[0003] In addition, the existing alumina polishing liquid usually contains too many chemical reagents and is complicated to prepare. For example, the patent application CN115029070A discloses a method for preparing alumina polishing liquid for C-type sapphire. Although the prepared alumina polishing liquid greatly increases the polishing rate, too many reagents are added; and there is a hydrogen peroxide oxidant, which affects the effect under alkaline conditions. The oxidant added with hydrogen peroxide is relatively easy to decompose, and the added hydrogen peroxide is easy to volatilize, and the barrel will swell. Another example is an alumina polishing liquid for polishing sapphire and its preparation method disclosed in patent CN114456716. Although the prepared alumina polishing liquid has high suspension dispersibility and good wettability, hydrogen peroxide oxidant is also added. The hydrogen peroxide oxidant added to the alumina polishing liquid will lose its effect after a period of preparation due to its volatility, and needs to be added on site, which brings a burden to production. Summary of the invention

[0004] The purpose of the present invention is to provide a sapphire substrate alumina polishing liquid to solve the problems of poor dispersibility, low polishing efficiency and excessive addition of chemical reagents in the prior art of alumina polishing liquid for sapphire substrates, which is not conducive to improving the use efficiency. The sapphire substrate alumina polishing liquid is prepared by using a macromolecular dispersant to disperse fine-grained alumina powder, has good suspension, less chemical reagents are added, and has high polishing efficiency.

[0005] The present invention also aims to provide a method for preparing the above-mentioned sapphire substrate sheet aluminum oxide polishing liquid.

[0006] The purpose of the present invention is achieved through the following technical solutions.

[0007] A sapphire substrate sheet alumina polishing liquid consists of the following components by mass percentage: 20-30% alumina powder, 1-5% macromolecular dispersant, 1-10% polishing accelerator, 1-3% pH regulator, and the balance is water; the macromolecular dispersant is a mixture of any one or more of sorbitol, sodium lauryl sulfate, sodium lignin sulfonate, polyvinyl alcohol, sodium methacrylate, ethylene glycol monobutyl ether and propylene glycol methyl ether acetate.

[0008] In a preferred embodiment, the alumina powder is α-alumina powder.

[0009] In a preferred embodiment, the particle size of the alumina powder is 0.5-1.0 μm.

[0010] In a preferred embodiment, the pH value of the sapphire substrate aluminum oxide polishing liquid is 9-13.

[0011] In a preferred embodiment, the polishing accelerator includes a mixture of any one or more of polyethylene glycol 400, fatty alcohol polyoxyethylene ether, glycerol and polyvinyl alcohol.

[0012] In a preferred embodiment, the pH adjuster is a mixture of any one or more of sodium hydroxide, ethanolamine, diethanolamine, potassium hydroxide and tetramethylammonium hydroxide, more preferably tetramethylammonium hydroxide.

[0013] In a preferred embodiment, the sapphire substrate alumina polishing liquid is composed of the following components by mass percentage: 20% alumina powder, 1% macromolecular dispersant, 1% polishing accelerator, 1-3% pH regulator, and the balance is water.

[0014] In a preferred embodiment, the sapphire substrate alumina polishing liquid is characterized in that, by mass percentage, it is composed of the following components: 20% alumina powder, 1% macromolecular dispersant, the macromolecular dispersant is sorbitol, 1% polishing accelerator, the polishing accelerator is polyvinyl alcohol, 1-3% pH adjuster, and the balance is water.

[0015] The method for preparing the alumina polishing liquid for a sapphire substrate described in any one of the above items comprises the following steps:

[0016] (1) dispersing the alumina powder in water to form an alumina powder solution;

[0017] (2) under stirring conditions, the polishing accelerator and the macromolecular dispersant are sequentially added to the alumina powder solution, and stirred to dissolve evenly;

[0018] (3) Add the pH adjuster and continue stirring until the mixture is uniform, thereby obtaining the sapphire substrate sheet aluminum oxide polishing liquid.

[0019] Preferably, in step (2), the stirring speed is 1000-1500 r / min.

[0020] Preferably, in step (3), the stirring is continued for 10-30 minutes.

[0021] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0022] The sapphire substrate sheet aluminum oxide polishing liquid of the present invention is composed of aluminum oxide powder, macromolecular dispersant, polishing accelerator, pH regulator and water. The macromolecular dispersant can well disperse the aluminum oxide powder, so that the aluminum oxide powder particles in the polishing liquid are evenly distributed, thereby maximizing the polishing performance of the polishing liquid and improving the polishing rate of the polishing liquid, and the aluminum oxide powder is a fine-grained particle powder. Therefore, when the substrate sheet is used for polishing, it is not easy to cause scratches, the surface roughness Ra can reach less than 0.3nm, the removal rate can reach more than 15μm / h, and it has excellent polishing efficiency.

[0023] In addition, no hydrogen peroxide oxidant is added to the alumina polishing liquid for the sapphire substrate, which not only ensures good dispersibility of the polishing liquid, but also avoids the problems of poor suspension of alumina powder and ineffectiveness of the polishing liquid caused by the volatilization of hydrogen peroxide, and makes the polishing liquid easy to store and use, reduces costs, and has a high cost-effectiveness.

[0024] The method for preparing the sapphire substrate sheet aluminum oxide polishing liquid of the present invention adopts a specific process to mix the components based on the characteristics of the various components of the sapphire substrate sheet aluminum oxide polishing liquid to obtain the sapphire substrate sheet aluminum oxide polishing liquid with high dispersion uniformity and good dispersion stability, thereby realizing the large-scale production of the sapphire substrate sheet aluminum oxide polishing liquid. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is an electron microscope image of the aluminum oxide powder used in the specific embodiment;

[0026] Figure 2 is a particle size distribution diagram of the alumina powder used in the specific embodiment;

[0027] Figure 3 This is an observation diagram of the surface roughness of a sapphire substrate after being polished with the alumina polishing liquid of Example 1. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments, but the protection scope and implementation mode of the present invention are not limited thereto. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0029] And, unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0030] It should be understood that the singular forms used in the present invention, such as "a", include plural references unless otherwise specified. In addition, the terms "including", "containing", and "having" are open-ended definitions rather than closed-ended definitions, that is, they include the contents specified in the present invention, but do not exclude other aspects. In other words, the terms also include "essentially consisting of" or "consisting of".

[0031] In addition, "and combinations thereof" in the specification refers to any combination of all listed items. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0032] Unless otherwise specified, all technical and scientific terms used herein have the standard meaning in the field to which the claimed subject matter belongs. If there are multiple definitions for a term, the definition herein shall prevail.

[0033] Unless otherwise indicated, this invention employs standard nomenclature and standard laboratory procedures and techniques of analytical chemistry, synthetic organic chemistry, and optics.

[0034] Without violating the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0035] In the following specific examples, some of the raw materials used and their sources are as follows:

[0036] Alumina powder, Tianjin Damao Chemical Reagent Factory;

[0037] Sodium lignin sulfonate, Tianjin Damao Chemical Reagent Factory;

[0038] Sorbitol, Tianjin Damao Chemical Reagent Factory;

[0039] Fatty alcohol polyoxyethylene ether, Tianjin Damao Chemical Reagent Factory;

[0040] Polyvinyl alcohol, Tianjin Damao Chemical Reagent Factory.

[0041] In a specific embodiment, the electron microscope image and particle size distribution of the aluminum oxide powder used are as follows: Figure 1 and Figure 2 As shown. Among them, from Figure 1 It can be seen from the figure that alumina powder is a granular powder with full and uniform particles, so it has a large cutting force. On the other hand, the powder particles do not have large edges and corners, and will not cause large scratches on the sapphire substrate during polishing. Figure 2It can be seen that the particle size distribution of the aluminum oxide powder used is uniform, and the main particle size distribution of the particles is 0.5-1.0 microns (D10-D50). Therefore, during the polishing process of the polishing liquid, a high removal rate can be provided, and the surface of the substrate will not have large deep scratches, forming a lower roughness and a smooth surface.

[0042] The technical solution of the present invention is described in detail below in conjunction with specific embodiments.

[0043] Example 1

[0044] The sapphire substrate alumina polishing liquid of this embodiment has a pH value of 9.0 and is composed of the following components by mass percentage: 20% alumina powder, 1% sodium lignin sulfonate, 1% fatty alcohol polyoxyethylene ether, 1% potassium hydroxide, and the rest is distilled water.

[0045] The steps for preparing the alumina polishing liquid for the sapphire substrate of this embodiment are as follows:

[0046] (1) Weigh each raw material component according to mass percentage;

[0047] (2) dispersing alumina powder in distilled water to form an alumina powder solution; adding fatty alcohol polyoxyethylene ether and sodium lignin sulfonate to the alumina powder solution in sequence under stirring at 1000 r / min, and stirring to uniformly dissolve;

[0048] (3) Add potassium hydroxide and continue stirring for 10 minutes until the mixture is uniformly mixed, and adjust the pH value to 9.0 to obtain the aluminum oxide polishing liquid for the sapphire substrate of this embodiment.

[0049] Example 2

[0050] The sapphire substrate alumina polishing liquid of this embodiment has a pH value of 9.0 and is composed of the following components by mass percentage: 20% alumina powder, 1.5% sodium lignin sulfonate, 2% fatty alcohol polyoxyethylene ether, 1% potassium hydroxide, and the rest is distilled water.

[0051] The steps for preparing the alumina polishing liquid for the sapphire substrate of this embodiment are as follows:

[0052] (1) Weigh each raw material component according to mass percentage;

[0053] (2) dispersing alumina powder in distilled water to form an alumina powder solution; adding fatty alcohol polyoxyethylene ether and sodium lignin sulfonate to the alumina powder solution in sequence under stirring at 1000 r / min, and stirring to uniformly dissolve;

[0054] (3) Add potassium hydroxide and continue stirring for 10 minutes until the mixture is uniformly mixed, and adjust the pH value to 9.0 to obtain the aluminum oxide polishing liquid for the sapphire substrate of this embodiment.

[0055] Example 3

[0056] The sapphire substrate alumina polishing liquid of this embodiment has a pH value of 10.0 and is composed of the following components by mass percentage: 25% alumina powder, 2.0% sodium lignin sulfonate, 4% fatty alcohol polyoxyethylene ether, 1% potassium hydroxide, and the rest is distilled water.

[0057] The steps for preparing the alumina polishing liquid for the sapphire substrate of this embodiment are as follows:

[0058] (1) Weigh each raw material component according to mass percentage;

[0059] (2) dispersing alumina powder in distilled water to form an alumina powder solution; adding fatty alcohol polyoxyethylene ether and sodium lignin sulfonate to the alumina powder solution in sequence under stirring at 1000 r / min, and stirring to uniformly dissolve;

[0060] (3) Add potassium hydroxide and continue stirring for 10 minutes until the mixture is uniformly mixed, and adjust the pH value to 10.0 to obtain the aluminum oxide polishing liquid for the sapphire substrate of this embodiment.

[0061] Example 4

[0062] The sapphire substrate alumina polishing liquid of this embodiment has a pH value of 11.0 and is composed of the following components by mass percentage: 25% alumina powder, 3.0% sodium lignin sulfonate, 6% fatty alcohol polyoxyethylene ether, 2% potassium hydroxide, and the rest is distilled water.

[0063] The steps for preparing the alumina polishing liquid for the sapphire substrate of this embodiment are as follows:

[0064] (1) Weigh each raw material component according to mass percentage;

[0065] (2) dispersing alumina powder in distilled water to form an alumina powder solution; adding fatty alcohol polyoxyethylene ether and sodium lignin sulfonate to the alumina powder solution in sequence under stirring at 1200 r / min, and stirring to uniformly dissolve;

[0066] (3) Add potassium hydroxide and continue stirring for 10 minutes until the mixture is uniformly mixed, and adjust the pH value to 11.0 to obtain the aluminum oxide polishing liquid for the sapphire substrate of this embodiment.

[0067] Example 5

[0068] The sapphire substrate alumina polishing liquid of this embodiment has a pH value of 12.0 and is composed of the following components by mass percentage: 30% alumina powder, 4.0% sodium lignin sulfonate, 8% fatty alcohol polyoxyethylene ether, 2% potassium hydroxide, and the rest is distilled water.

[0069] The steps for preparing the alumina polishing liquid for the sapphire substrate of this embodiment are as follows:

[0070] (1) Weigh each raw material component according to mass percentage;

[0071] (2) dispersing alumina powder in distilled water to form an alumina powder solution; adding fatty alcohol polyoxyethylene ether and sodium lignin sulfonate to the alumina powder solution in sequence under stirring at 1200 r / min, and stirring to uniformly dissolve;

[0072] (3) Add potassium hydroxide and continue stirring for 10 minutes until the mixture is uniformly mixed, and adjust the pH value to 12.0 to obtain the aluminum oxide polishing liquid for the sapphire substrate of this embodiment.

[0073] Example 6

[0074] The sapphire substrate alumina polishing liquid of this embodiment has a pH value of 13.0 and is composed of the following components by mass percentage: 30% alumina powder, 2.0% sodium lignin sulfonate, 10% fatty alcohol polyoxyethylene ether, 2% potassium hydroxide, and the rest is distilled water.

[0075] The steps for preparing the alumina polishing liquid for the sapphire substrate of this embodiment are as follows:

[0076] (1) Weigh each raw material component according to mass percentage;

[0077] (2) dispersing alumina powder in distilled water to form an alumina powder solution; adding fatty alcohol polyoxyethylene ether and sodium lignin sulfonate to the alumina powder solution in sequence under stirring at 1200 r / min, and stirring to uniformly dissolve;

[0078] (3) Add potassium hydroxide and continue stirring for 10 minutes until the mixture is uniformly mixed, and adjust the pH value to 13.0 to obtain the aluminum oxide polishing liquid for the sapphire substrate of this embodiment.

[0079] Example 7

[0080] The sapphire substrate alumina polishing liquid of this embodiment has a pH value of 9.0. The sapphire substrate alumina polishing liquid is composed of the following components by mass percentage: 20% alumina powder, 1% sorbitol, 1% polyvinyl alcohol, 3% potassium hydroxide, and the rest is distilled water.

[0081] The steps for preparing the alumina polishing liquid for the sapphire substrate of this embodiment are as follows:

[0082] (1) Weigh each raw material component according to mass percentage;

[0083] (2) dispersing alumina powder in distilled water to form an alumina powder solution; adding polyvinyl alcohol and sorbitol to the alumina powder solution in sequence under stirring at 1500 r / min, and stirring to uniformly dissolve;

[0084] (3) Add potassium hydroxide and continue stirring for 10 minutes until the mixture is uniformly mixed, and adjust the pH value to 9.0 to obtain the aluminum oxide polishing liquid for the sapphire substrate of this embodiment.

[0085] Example 8

[0086] The sapphire substrate alumina polishing liquid of this embodiment has a pH value of 11.0. The sapphire substrate alumina polishing liquid is composed of the following components by mass percentage: 25% alumina powder, 3.0% sorbitol, 5% polyvinyl alcohol, 3% potassium hydroxide, and the rest is distilled water.

[0087] The steps for preparing the alumina polishing liquid for the sapphire substrate of this embodiment are as follows:

[0088] (1) Weigh each raw material component according to mass percentage;

[0089] (2) dispersing alumina powder in distilled water to form an alumina powder solution; adding polyvinyl alcohol and sorbitol to the alumina powder solution in sequence under stirring at 1500 r / min, and stirring to uniformly dissolve;

[0090] (3) Add potassium hydroxide and continue stirring for 10 minutes until the mixture is uniformly mixed, and adjust the pH value to 11.0 to obtain the aluminum oxide polishing liquid for the sapphire substrate of this embodiment.

[0091] Example 9

[0092] The sapphire substrate alumina polishing liquid of this embodiment has a pH value of 13.0. The sapphire substrate alumina polishing liquid is composed of the following components by mass percentage: 30% alumina powder, 5.0% sorbitol, 10% polyvinyl alcohol, 3% potassium hydroxide, and the rest is distilled water.

[0093] The steps for preparing the alumina polishing liquid for the sapphire substrate of this embodiment are as follows:

[0094] (1) Weigh each raw material component according to mass percentage;

[0095] (2) dispersing alumina powder in distilled water to form an alumina powder solution; adding polyvinyl alcohol and sorbitol to the alumina powder solution in sequence under stirring at 1500 r / min, and stirring to uniformly dissolve;

[0096] (3) Add potassium hydroxide and continue stirring for 10 minutes until the mixture is uniformly mixed, and adjust the pH value to 13.0 to obtain the aluminum oxide polishing liquid for the sapphire substrate of this embodiment.

[0097] Comparative Example 1

[0098] Alumina polishing liquid commonly used on the market, Suzhou Xindong Technology Co., Ltd.

[0099] Comparative Example 2

[0100] The raw material components and preparation method of the sapphire substrate alumina polishing liquid of this comparative example are the same as those of Example 1, except that the particle size of the alumina powder is selected to be 0.1-0.3 μm.

[0101] Comparative Example 3

[0102] The raw material components and preparation method of the sapphire substrate alumina polishing liquid of this comparative example are the same as those of Example 1, except that the particle size of the alumina powder is selected to be 2.0-2.5 μm.

[0103] Comparative Example 4

[0104] The raw material components and preparation method of the sapphire substrate alumina polishing liquid of this comparative example are similar to those of Example 1, except that the content of alumina powder is 15%.

[0105] 1. Polishing test

[0106] Experimental conditions:

[0107] Material: 4-inch sapphire substrate

[0108] Machine: Shenzhen Fufengyuan 610# polishing machine

[0109] Polishing pad: Imported SUBA600 polishing pad

[0110] Polishing time: 60min (cycle)

[0111] Polishing pressure: 180g / cm 2

[0112] Polishing liquid flow rate: 60ml / min

[0113] The surface roughness Ra of the sapphire substrate after the polishing test using the sapphire substrate alumina polishing liquid of Example 1 is as follows: Figure 3 As shown by Figure 3It can be seen that the roughness Ra of the polished sapphire substrate is 0.27 nm.

[0114] The polishing test results of the sapphire substrate sheets of Examples 1-9 and Comparative Examples 1-4 using the alumina polishing liquid are shown in Table 1 below.

[0115] Table 1 Polishing test results of the polishing liquids of Examples 1-9 and Comparative Examples 1-2

[0116]

[0117]

[0118] It can be seen from the test results in Table 1 that the sapphire substrate alumina polishing liquids of Examples 1-9 have higher polishing rates and lower surface roughness than the sapphire substrate alumina polishing liquids of Comparative Examples 1-4. Among them, compared with Examples 1-9, the commercially available sapphire substrate alumina polishing liquid of Comparative Example 1 has a rapid failure and a serious reduction in polishing rate due to the volatile components added, etc.; when Comparative Example 2 uses a finer particle size of 0.1-0.3μm alumina powder, the removal rate is low and the surface effect is poor. The reason is that the powder particle size is small, the friction is small, the friction between the powder and the polishing skin is small, the cutting force acting on the product is insufficient, and there are residual scratches on the surface; and when Comparative Example 3 uses a coarser particle size of 2.0-2.5μm alumina powder, a higher removal rate can be achieved, but the surface roughness is also high, because the powder particle size is large, the number of large particles acting on a unit area is large, and scratches are easily formed; when the sapphire substrate alumina polishing liquid of Comparative Example 4 has a low content of alumina powder, the number of powder particles that play a grinding role is reduced, and the relative removal rate is reduced. The same removal rate cannot meet the requirements, the scratches on the surface cannot be removed, and the surface roughness is also relatively large.

[0119] In summary, the experimental results show that the sapphire substrate alumina polishing liquid of the present invention has good dispersibility and high removal rate under the condition of strictly controlling the content of each component and the selection of raw materials, especially when the percentage content of alumina powder is 20-30%, the particle size of alumina powder is 0.5-1.0μm and a macromolecular dispersant is used. The macromolecular non-ionic dispersant can make the alumina powder well dispersed, the particles are uniform, and the polishing performance of the polishing liquid is maximized, the polishing rate of the polishing liquid is improved, there are no scratches caused by particles on the surface, the surface Ra can reach 0.2nm-0.3nm, the removal rate can reach more than 15μm / h, the alumina powder does not precipitate, the dispersibility is good, and each particle can play a maximum role to achieve the best effect.

[0120] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, this specification does not describe all possible combinations of the technical features in the above-mentioned embodiments. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. Moreover, the above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as a limitation on the scope of the invention patent.

[0121] It should be noted that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these modifications and improvements all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A sapphire substrate aluminum oxide polishing liquid, characterized in that: The invention is composed of the following components by mass percentage: 20-30% alumina powder, 1-5% macromolecular dispersant, 1-10% polishing accelerator, 1-3% pH regulator, and the balance is water; the macromolecular dispersant is a mixture of any one or more of sorbitol, sodium lauryl sulfate, sodium lignin sulfonate, polyvinyl alcohol, sodium methacrylate, ethylene glycol monobutyl ether and propylene glycol methyl ether acetate; The particle size of the alumina powder is 0.5-1.0 μm; the alumina powder is α-alumina powder; The polishing accelerator includes a mixture of any one or more of polyethylene glycol 400, fatty alcohol polyoxyethylene ether, glycerol and polyvinyl alcohol; The pH regulator is a mixture of any one or more of sodium hydroxide, ethanolamine, diethanolamine, potassium hydroxide and tetramethylammonium hydroxide.

2. The sapphire substrate aluminum oxide polishing liquid according to claim 1, characterized in that: The pH value is 9-13.

3. The sapphire substrate aluminum oxide polishing liquid according to any one of claims 1 to 2, characterized in that: The composition is as follows by mass percentage: 20% alumina powder, 1% macromolecular dispersant, 1% polishing accelerator, 1-3% pH regulator, and the balance is water.

4. The sapphire substrate aluminum oxide polishing liquid according to claim 1, characterized in that: The invention is composed of the following components by mass percentage: 20% alumina powder, 1% macromolecular dispersant, wherein the macromolecular dispersant is sorbitol, 1% polishing accelerator, wherein the polishing accelerator is polyvinyl alcohol, 1-3% pH regulator, and the balance is water.

5. A method for preparing the sapphire substrate aluminum oxide polishing liquid according to any one of claims 1 to 4, characterized in that: The steps include: (1) dispersing the alumina powder in water to form an alumina powder solution; (2) Under stirring conditions, the polishing accelerator and the macromolecular dispersant are sequentially added to the alumina powder solution, and stirred to dissolve evenly; (3) Add the pH adjuster and continue stirring until the mixture is uniformly mixed to obtain the sapphire substrate sheet aluminum oxide polishing liquid.

6. The preparation method according to claim 5, characterized in that: In step (2), the stirring speed is 1000-1500 r / min.

7. The preparation method according to claim 5, characterized in that: In step (3), the stirring time is 10-30 minutes.

Citation Information

Patent Citations

  • Preparation method of aluminum oxide polishing solution for C-direction sapphire

    CN115029070A

  • High-performance sapphire grinding fluid and preparation method thereof

    CN104592898A

  • High-efficiency mixed abrasive chemical mechanical polishing solution for sapphire substrate

    CN110511679A