A medium-low temperature water-boiled glue suitable for cutting large-size silicon wafers

By grafting and modifying polythiol with N-acryloylmorpholine, the problems of high wafer dropping rate and difficulty in degumming at medium and low temperatures in large-size silicon wafers are solved, achieving high bonding strength and low power. The low-cost glue reduces the contamination rate of the glue surface.

CN116376494BActive Publication Date: 2024-10-29WUHAN YITIAN SCI&TECH DEV CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202111585342.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-23
Publication Date
2024-10-29
Estimated Expiration
2041-12-23

AI Technical Summary

Technical Problem

Existing silicon wafer cutting adhesives have a high rate of chip removal during large-size silicon wafer cutting, and existing methods cannot effectively degumming at medium and low temperatures, resulting in high power costs and a high rate of contamination of the adhesive surface.

Method used

By grafting and modifying polythiol with N-acryloylmorpholine, the bonding strength of the adhesive is increased, and degumming without acid boiling is achieved at medium and low temperatures, making use of the hydrophilicity and catalytic effect of the morpholine group. , reduce the adhesive force between the glue layer and the silicon wafer, and enhance the solidification of the glue layer.

Benefits of technology

It achieves effective degumming at medium and low temperatures below 60°C, reduces the chip drop rate and electricity costs, reduces the amount of catalyst, and improves the environmental protection and energy saving of the glue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure DEST_PATH_IMAGE001
    Figure DEST_PATH_IMAGE001
Patent Text Reader

Abstract

The present invention belongs to a special two-component epoxy adhesive suitable for silicon rod cutting, and particularly relates to a medium-low temperature water-boiled adhesive suitable for large-size silicon wafer cutting and a preparation method thereof, wherein the water-boiled adhesive raw materials include epoxy resin, N-acryloylmorpholine modified polythiol, filler, defoamer, pigment, anti-settling agent, accelerator, etc., and the N-acryloylmorpholine modified polythiol is a special monomer of N-acryloylmorpholine, and polythiol is grafted and modified. The adhesive provided by the present invention is more suitable for large-size silicon wafer cutting than commercially available adhesives, has a low chip drop rate, can achieve water-boiled degumming without adding an acidic degumming agent, is more environmentally friendly, and can be degummed at medium and low temperatures, which is more energy-saving.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to glue used in a silicon rod cutting process in the photovoltaic industry, and in particular to a medium-low temperature water-boiled glue suitable for cutting large-size silicon wafers. Background Art

[0002] The silicon rod bonding glue suitable for the silicon wafer cutting process is a two-component epoxy adhesive. At the silicon wafer cutting process end, due to the increasing size of silicon wafers at this stage, the adhesives on the market often fall off during the cutting process, so the bonding strength of the adhesive is required to be higher and higher. After the silicon wafer is cut, the silicon wafer needs to be placed in the debonding tank for debonding. Lactic acid debonding agent needs to be added to the debonding tank, and it needs to be boiled at 60-80℃ for 400-800s before debonding. Nowadays, single crystals are the mainstream of the market. Compared with polycrystalline, they have higher requirements for silicon rod cutting adhesives. At the debonding process end, the debonding temperature needs to be reduced to below 60℃. Therefore, the market needs a stick adhesive with high bonding strength that can be debonded at medium and low temperatures below 60℃ without adding acid and boiling.

[0003] In the prior art, patent CN109321185A discloses that in order to improve the bonding strength, the epoxy resin and the polythiol curing agent are treated with ultraviolet light; in order to achieve degumming without adding acid, sodium polyacrylate or polyacrylamide degumming factors are added to the filler, and other patents also mention the addition of microsphere expansion agents to degumming the adhesive by boiling. This type of method for achieving degumming without adding acid is to add some sodium polyacrylate-type water-absorbing resin or microsphere expansion agent, and achieve degumming through the physical method of water absorption and expansion of the water-absorbing resin or heat absorption and expansion of the microsphere expansion agent. This type of method has certain limitations in single crystal cutting today. Since the back-end texturing process of single crystal silicon wafers and multi-crystalline silicon wafers is different, single crystal silicon wafers have higher requirements for surface cleanliness. Therefore, the degumming process temperature is required to be 60°C or even lower to reduce the dirt rate of the silicon wafer's adhesive surface. When heated, a small amount of low-molecular-weight resins such as sodium polyacrylate will dissolve or swell, and flow to the surface of the silicon wafer, resulting in a high rate of dirt on the adhesive surface of the silicon wafer. The minimum expansion temperature of the microsphere expansion agent is 75°C. To achieve water degumming, the temperature needs to be raised to 80°C. The high degumming temperature not only leads to high electricity costs, but also causes the amine catalyst that has not fully reacted in the adhesive layer to flow to the silicon wafer, resulting in a high rate of dirt on the adhesive surface of the silicon wafer.

[0004] The present invention provides a silicon rod cutting adhesive with a chemically modified curing agent to increase the bonding strength of the adhesive so as to be more suitable for large-size silicon wafer cutting and achieve the purpose of debonding at a medium or low temperature below 60°C without adding acid and boiling. Summary of the invention

[0005] The sticky glue currently used for silicon wafer cutting on the market is an epoxy / polythiol (Capcure-3800) curing system, in which a certain amount of fillers, accelerators, etc. are added. The current sticky glue system cannot be debonded well at medium and low temperatures below 60°C without acid boiling, and when used for cutting large-size silicon wafers, the chip drop rate is high, and it is not suitable for cutting large-size silicon wafers.

[0006] The purpose of the present invention is to solve the above problems and provide a medium-low temperature water-boiled glue suitable for cutting large-size silicon wafers and a preparation method thereof. The medium-low temperature water-boiled glue suitable for cutting large-size silicon wafers provided by the present invention is characterized by the following composition (by weight):

[0007] Component A: 50-80 parts of epoxy resin, 20-50 parts of filler, 0.1-1 parts of anti-settling agent, and 0.01-1 parts of defoaming agent.

[0008] Component B: 50-80 parts of N-acryloylmorpholine grafted modified polythiol, 0.1-5 parts of accelerator, 20-50 parts of filler, 0.1-1 parts of anti-settling agent, 0.01-1 parts of defoaming agent, and 0.01-1 parts of pigment.

[0009] Wherein, the epoxy resin is one or more of the general epoxy resins 127, 128, and 170.

[0010] The filler is one or more of calcium carbonate, aluminum hydroxide, quartz powder, titanium dioxide, and talcum powder.

[0011] The anti-settling agent is one or more of fumed silica and castor oil derivatives.

[0012] The defoaming agent is one or more of tego900, teg930, and tego931.

[0013] The accelerator is one or more of DMP-30, triethanolamine, dimethylbenzylamine and triethylenetetramine.

[0014] The pigment is one of phthalocyanine blue, phthalocyanine green and scarlet powder.

[0015] The N-acryloylmorpholine grafted modified polythiol is prepared by chemically modifying a multifunctional polythiol with N-acryloylmorpholine, wherein N-acryloylmorpholine is grafted into the polythiol, wherein the multifunctional polythiol is one or more of Cpacure-3800, trimethylolpropane tris(3-mercaptoacrylate), and pentaerythritol tetra(3-mercaptopropionic acid) ester.

[0016] The structural reaction formula of the N-acryloylmorpholine grafted modified polythiol is as follows:

[0017]

[0018] Where: n=3-4;

[0019] x>2 and x<n;

[0020] The preparation method of the N-acryloylmorpholine grafted modified polythiol is as follows: an excess amount of polythiol and a certain amount of N-acryloylmorpholine are added into a reaction kettle, stirred evenly, and then a catalyst of benzoin dimethyl ether is added, and the mixture is reacted for 30 minutes under ultraviolet light to obtain the N-acryloylmorpholine grafted modified polythiol curing agent.

[0021] The method for preparing a medium-low temperature water-boiled glue suitable for cutting large-size silicon wafers comprises the following steps:

[0022] (1) Preparation of component A: In a planetary stirred reactor, add epoxy resin and defoamer, stir for 10 min, then add filler and anti-settling agent in batches, and stir at 20-50°C for 2 h.

[0023] (2) Preparation method of component B: In a planetary stirred reactor, add N-acryloylmorpholine grafted modified polythiol and accelerator, stir for 30 minutes, then add defoamer and stir for 10 minutes, finally add pigment, filler and anti-settling agent in batches, and stir at 20-50°C for 2 hours.

[0024] The invention has the advantages that: by chemically modifying the polythiol (Capcure-38000 or polythioacrylate) currently used for silicon rod bonding on the market, N-acryloylmorpholine is grafted onto the polythiol. Since the morpholine group in N-acryloylmorpholine has good hydrophilicity and hygroscopicity, when the glue layer is debonded after curing, water molecules are more likely to penetrate into the glue layer, destroy the hydrogen bond between the glue layer and the silicon wafer, and reduce the bonding force between the glue layer and the silicon wafer, so that good debonding can be achieved under medium and low temperature or even room temperature without adding acid. In addition, the NH bond in the morpholine group is easier to form a hydrogen bond with the oxide layer on the silicon wafer, so that the bonding strength of the glue layer to the silicon wafer can be enhanced. At the same time, the secondary amine in the morpholine group has a catalytic effect on the polythiol, which can reduce the amount of the catalyst. Therefore, by grafting N-acryloylmorpholine into the polythiol curing agent, not only can the bonding strength of the glue to the silicon wafer be enhanced, but also the glue can be debonded under medium and low temperature without adding acid. At the same time, it can reduce the amount of catalyst used, making the glue more environmentally friendly and energy-saving. DETAILED DESCRIPTION

[0025] The technical scheme of the present invention is further described in detail below through examples, but the scope of the present invention is not limited in any way.

[0026] Example 1

[0027] The preparation method of N-acryloylmorpholine grafted modified polythiol is as follows: add 90 parts of polythiol Capcure-3800, 10 parts of trimethylolpropane tris (3-mercaptoacrylate), and 20 parts of N-acryloylmorpholine into a reactor, stir evenly, then add 2 parts of catalyst benzoin dimethyl ether, react for 30 minutes under ultraviolet light, and obtain N-acryloylmorpholine grafted modified polythiol curing agent.

[0028] A method for preparing medium-low temperature water-boiled glue suitable for cutting large-size silicon wafers comprises the following steps:

[0029] (1) Preparation method of component A: In a planetary stirred reactor, add 70 parts of epoxy resin E51 and 0.5 parts of defoaming agent Tego900, stir for 10 minutes, then add 30 parts of calcium carbonate filler and 1 part of fumed silica in batches, and stir at 20-50°C for 2 hours.

[0030] (2) Preparation method of component B: In a planetary stirred reactor, add 70 parts of the above-mentioned N-acryloylmorpholine grafted modified polythiol and 2 parts of DMP-30 accelerator, stir for 30 minutes, then add 0.5 parts of defoaming agent tego900 and stir for 10 minutes, finally add 0.05 parts of pigment phthalocyanine blue, 30 parts of calcium carbonate filler, and 1 part of fumed silica in batches, and stir at 20-50°C for 2 hours.

[0031] Example 2

[0032] The preparation method of N-acryloylmorpholine grafted modified polythiol is as follows: add 90 parts of polythiol Capcure-3800, 10 parts of trimethylolpropane tris (3-mercaptoacrylate), and 16 parts of N-acryloylmorpholine into a reactor, stir evenly, then add 2 parts of catalyst benzoin dimethyl ether, react for 30 minutes under ultraviolet light, and obtain N-acryloylmorpholine grafted modified polythiol curing agent.

[0033] A method for preparing medium-low temperature water-boiled glue suitable for cutting large-size silicon wafers comprises the following steps:

[0034] (1) Preparation method of component A: In a planetary stirred reactor, add 70 parts of epoxy resin E51 and 0.5 parts of defoaming agent Tego900, stir for 10 minutes, then add 30 parts of calcium carbonate filler and 1 part of fumed silica in batches, and stir at 20-50°C for 2 hours.

[0035] (2) Preparation method of component B: In a planetary stirred reactor, add 70 parts of the above-mentioned N-acryloylmorpholine grafted modified polythiol and 2 parts of DMP-30 accelerator, stir for 30 minutes, then add 0.5 parts of defoaming agent tego900 and stir for 10 minutes, finally add 0.05 parts of pigment phthalocyanine blue, 30 parts of calcium carbonate filler, and 1 part of fumed silica in batches, and stir at 20-50°C for 2 hours.

[0036] Example 3

[0037] The preparation method of N-acryloylmorpholine grafted modified polythiol is as follows: add 90 parts of polythiol Capcure-3800, 10 parts of trimethylolpropane tris (3-mercaptoacrylate), and 8 parts of N-acryloylmorpholine into a reactor, stir evenly, then add 2 parts of catalyst benzoin dimethyl ether, react for 30 minutes under ultraviolet light, and obtain N-acryloylmorpholine grafted modified polythiol curing agent.

[0038] A method for preparing medium-low temperature water-boiled glue suitable for cutting large-size silicon wafers comprises the following steps:

[0039] (1) Preparation method of component A: In a planetary stirred reactor, add 70 parts of epoxy resin E51 and 0.5 parts of defoaming agent Tego900, stir for 10 minutes, then add 30 parts of calcium carbonate filler and 1 part of fumed silica in batches, and stir at 20-50°C for 2 hours.

[0040] (2) Preparation method of component B: In a planetary stirred reactor, add 70 parts of the above-mentioned N-acryloylmorpholine grafted modified polythiol and 2 parts of DMP-30 accelerator, stir for 30 minutes, then add 0.5 parts of defoaming agent tego900 and stir for 10 minutes, finally add 0.05 parts of pigment phthalocyanine blue, 30 parts of calcium carbonate filler, and 1 part of fumed silica in batches, and stir at 20-50°C for 2 hours.

[0041] Example 4

[0042] The preparation method of N-acryloylmorpholine grafted modified polythiol is as follows: add 90 parts of polythiol Capcure-3800, 10 parts of trimethylolpropane tris (3-mercaptoacrylate), and 4 parts of N-acryloylmorpholine into a reactor, stir evenly, then add 2 parts of catalyst benzoin dimethyl ether, react for 30 minutes under ultraviolet light, and obtain N-acryloylmorpholine grafted modified polythiol curing agent.

[0043] A method for preparing medium-low temperature water-boiled glue suitable for cutting large-size silicon wafers comprises the following steps:

[0044] (1) Preparation method of component A: In a planetary stirred reactor, add 70 parts of epoxy resin E51 and 0.5 parts of defoaming agent Tego900, stir for 10 minutes, then add 30 parts of calcium carbonate filler and 1 part of fumed silica in batches, and stir at 20-50°C for 2 hours.

[0045] (2) Preparation method of component B: In a planetary stirred reactor, add 70 parts of the above-mentioned N-acryloylmorpholine grafted modified polythiol and 2 parts of DMP-30 accelerator, stir for 30 minutes, then add 0.5 parts of defoaming agent tego900 and stir for 10 minutes, finally add 0.05 parts of pigment phthalocyanine blue, 30 parts of calcium carbonate filler, and 1 part of fumed silica in batches, and stir at 20-50°C for 2 hours.

[0046] Performance Testing

[0047] The performance test of the glue in the embodiment was compared with that of commercially available glue, and the results are shown in Table 1 below:

[0048] Table 1

[0049] Tensile shear strength (MPa) Surface drying time (min) Hardness (D) Example 1 17.5 9 88 Example 2 16.7 15 88 Example 3 15.4 20 88 Example 4 14.9 32 89 Commercially available glue 14.2 15 89

[0050] The tensile shear strength in Table 1 was tested according to GB / T7124-2008, and the samples were cured at room temperature for 4 hours.

[0051] The surface drying time in Table 1 is tested according to GBT13477.5-2002.

[0052] The hardness in Table 1 was tested according to GBT2411-2008, and the samples were cured at room temperature for 4 hours.

[0053] The glue in the embodiment and the commercially available glue were used to cut a large silicon wafer of size 210, and the chip drop rate of on-site cutting was counted. The results are shown in Table 2 below:

[0054] Table 2

[0055] Drop rate (%) Example 1 1.2 Example 2 0.47 Example 3 0.07 Example 4 0.09 Commercially available glue 0.53

[0056] The glue in the embodiment and the commercially available glue were used to cut a large silicon wafer of size 210, and then a degumming experiment was carried out. The degumming time at different temperatures was tested without adding acid. The results are shown in Table 3 below:

[0057] Table 3

[0058] 35℃ 40℃ 50℃ 60℃ Example 1 2400s 800s 200s 60s Example 2 3100s 950s 270s 70s Example 3 —— 1500s 310s 130s Example 4 —— 3400s 450s 230s Commercially available glue —— —— —— 800s

[0059] The “——” in Table 3 indicates that 3600s failed to achieve debonding.

[0060] It can be seen from Table 1 that as the amount of N-acryloylmorpholine grafted onto the polythiol increases, the bonding strength of the glue cured by using it as a curing agent increases, and the surface drying time increases, but it has no significant effect on the hardness.

[0061] Combining Table 1 and Table 2, it can be seen that although the bonding strength of the glue increases after the content of N-acryloylmorpholine is added to the polythiol, it does not necessarily reduce the chip drop rate during silicon wafer cutting. This is because during the silicon wafer cutting process, the silicon rod will be sprayed with aqueous coolant, and the glue layer is in a humid working environment. If there are too many N-acryloylmorpholine groups grafted on the polythiol, the glue layer will have too good water absorption, and water molecules can quickly penetrate into the glue layer, resulting in a decrease in bonding strength during the cutting process, thereby increasing the chip drop rate. Therefore, the grafting rate of N-acryloylmorpholine needs to be controlled within a certain range.

[0062] It can be seen from Table 3 that as the grafting rate of N-acryloylmorpholine increases, the degumming time is shorter at the same temperature. When the grafting rate of N-acryloylmorpholine is high, degumming can also be achieved at 35°C. In summary, the silicon rod cutting adhesive prepared by grafting a suitable amount of N-acryloylmorpholine on the polythiol curing agent can achieve degumming under the conditions of medium and low temperatures below 60°C without adding acid, while enhancing the bonding strength of the adhesive to the silicon wafer and reducing the silicon wafer drop rate during the cutting process.

[0063] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the embodiments, it should be understood by those skilled in the art that any modification or equivalent replacement of the technical solutions of the present invention does not depart from the spirit or scope of the technical solutions of the present invention and should be included in the scope of the claims of the present invention.

Claims

1. A medium and low temperature water-boiled glue suitable for cutting large-size silicon wafers. It is characterized in that include: Component A includes: 50-80 parts of epoxy resin, 20-50 parts of filler, 0.1-1 parts of anti-settling agent, and 0.01-1 parts of defoaming agent; the epoxy resin is one or more of the general epoxy resins 127, 128, and 170; Component B includes: 50-80 parts of N-acryloylmorpholine grafted modified polythiol, 0.1-5 parts of accelerator, 20-50 parts of filler, 0.1-1 parts of anti-settling agent, 0.01-1 parts of defoamer, and 0.01-1 parts of pigment; The N-acryloylmorpholine grafted modified polythiol is obtained by chemically modifying a multifunctional polythiol with N-acryloylmorpholine, wherein N-acryloylmorpholine is grafted into the multifunctional polythiol, wherein the multifunctional polythiol is a multifunctional polythiol Capcure-3800 and trimethylolpropane tris(3-mercaptoacrylate); The structural reaction formula of the N-acryloylmorpholine grafted modified polythiol is as follows: Wherein: n = 3-4; x>2 and x<n; in: It is multifunctional polythiol Capcure-3800 and trimethylolpropane tris(3-mercaptoacrylate); The preparation method of the N-acryloylmorpholine grafted modified polythiol is as follows: 100 parts of multifunctional polythiol and 4-20 parts of N-acryloylmorpholine are added into a reaction kettle, stirred evenly, and then a catalyst of benzoin dimethyl ether is added, and the mixture is reacted for 30 minutes under ultraviolet light to obtain the N-acryloylmorpholine grafted modified polythiol; wherein the multifunctional polythiol is multifunctional polythiol Capcure-3800 and trimethylolpropane tris(3-mercaptoacrylate).

2. The medium-low temperature water-boiled glue suitable for cutting large-size silicon wafers according to claim 1, It is characterized in that The filler is one or more of calcium carbonate, aluminum hydroxide, quartz powder, titanium dioxide, and talcum powder.

3. The medium-low temperature water-boiled glue suitable for cutting large-size silicon wafers according to claim 1, It is characterized in that The anti-settling agent is one or more of fumed silica and castor oil derivatives.

4. The medium-low temperature water-boiled glue suitable for cutting large-size silicon wafers according to claim 1, It is characterized in that The defoaming agent is one or more of tego900, teg930, and tego931.

5. The medium-low temperature water-boiled glue suitable for cutting large-size silicon wafers according to claim 1, It is characterized in that The accelerator is one or more of DMP-30, triethanolamine, dimethylbenzylamine and triethylenetetramine.

6. The medium-low temperature water-boiled glue suitable for cutting large-size silicon wafers according to claim 1, It is characterized in that The pigment is one of phthalocyanine blue, phthalocyanine green and scarlet powder.

Citation Information

Patent Citations

  • Rod sticking glue capable of degumming through water boiling and preparation method thereof

    CN109321185A

  • LED-UV phototherapy glue scrubbing-free sealing layer glue and preparation method thereof

    CN105878054A

  • Multi-component UV-LED light-cured silk screen ink for glass substrate, and preparation method thereof