A smelting and purification method for Mg-Li-Zn-Er-Yb alloy for three-dimensional printing
Through multi-stage inert gas rotary spraying and three-stage flux refining methods, the problems of oxidation and impurity pollution during smelting of magnesium lithium alloys are solved, significantly improving the purity and performance of the alloy and reducing costs.
Patent Information
- Application Number
- CN202211561174.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-07
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-07
AI Technical Summary
The existing magnesium lithium alloys are prone to react with air and equipment during the smelting process, resulting in oxidation and impurity pollution, affecting the quality of the ingot. The existing refining process has problems such as inconvenient separation of flux and consumption of lithium elements.
The multi-stage inert gas rotary spraying and tertiary flux refining methods of Mg-Li-Zn-Er-Yb alloy are used to gradually remove inclusions in the alloy through temperature control and the use of refining fluxes to ensure melt purity.
It significantly reduces the slag content of magnesium lithium alloy, improves the mechanical properties and corrosion resistance, reduces the burn loss rate of lithium elements and the sedimentation rate of Er and Yb elements, and reduces the smelting cost.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a method for smelting and purifying a Mg-Li-Zn-Er-Yb alloy melt for three-dimensional printing. Background Art
[0002] Modern industry has an increasingly obvious demand for ultra-light and high-strength materials. Magnesium-lithium alloys have attracted close attention from scientists due to their significant advantages, such as low density (generally 1.25-1.65g / cm 3 , 1 / 3-1 / 2 lighter than ordinary magnesium alloys, 1 / 2 of aluminum alloys), high specific strength, high specific stiffness, good electromagnetic shielding performance and damping characteristics, and excellent cutting performance. Therefore, magnesium-lithium alloys are widely used in the fields of national defense, aerospace, automobiles and electronic products, and have a very broad market prospect.
[0003] At present, aerospace parts with complex structures and large sizes are mainly produced by casting. If magnesium-lithium alloys are to be used in such aerospace parts, magnesium-lithium alloy billets are generally made by casting and forging, and then many subsequent processes such as mechanical processing are carried out. The reserved processing allowance is large, the utilization rate of raw materials is very low, and the stocking cycle is long, which seriously restricts the development progress of the model. Additive manufacturing technology (3D printing) has the advantages of no molds, short manufacturing cycle, and low cost. It can provide more design ideas for the manufacturing of complex aerospace components, which is conducive to the rapid and effective coordination of "design-process-manufacturing".
[0004] 3D printing technology first requires high-quality magnesium-lithium alloy ingots. When magnesium-lithium alloys are melted and cast in an atmospheric environment, the magnesium and lithium in the alloy are very likely to react chemically with substances such as oxygen and water in the air, smelting equipment or raw materials, causing oxidation or even combustion losses of the alloy elements, and introducing impurities such as oxides and carbides of magnesium and lithium elements to contaminate the melt. At the same time, the raw materials of magnesium-lithium alloys also contain a certain amount of inclusions. These impurities significantly reduce the mechanical properties and corrosion resistance of magnesium-lithium alloys. Therefore, during the smelting process of magnesium-lithium alloys, the melt must be refined and purified to remove inclusions in the melt and prevent the inclusions from affecting the quality of the ingot. The refining process of magnesium-lithium alloys studied at present is mainly flux refining, and the refining flux used is mainly lithium chloride and lithium fluoride flux (such as Yao Xinzhao, Research on the Melting and Casting Process and Microstructure Properties of Magnesium-Lithium Alloys [M], Master's Thesis of Hunan University in 2006, P1-32.). However, the flux is inconvenient to separate from the melt during the refining process, and flux inclusions are easily formed, which increases the contamination of the melt and affects the quality of the ingot. If ordinary magnesium alloy flux is used (such as Liu Wanghanbo, et al. Research Progress in Purification Technology of Magnesium Alloy Melts [J], Foundry, 2015, 64(6) P521-527.), lithium will react with the main component magnesium chloride, consume the lithium element in the melt, and cause instability in the composition of the ingot. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a smelting and purification method of Mg-Li-Zn-Er-Yb alloy for three-dimensional printing, reduce the slag content of the Mg-Li-Zn-Er-Yb alloy, and ensure the purity of the ingot.
[0006] The present invention provides a smelting and purification method of a Mg-Li-Zn-Er-Yb alloy for three-dimensional printing, comprising the following steps:
[0007] According to the composition of the Mg-Li-Zn-Er-Yb alloy, a magnesium source is melted to obtain a magnesium melt, and a zinc source is added and melted when the temperature of the magnesium melt is 680-700° C. to obtain a Mg-Zn melt;
[0008] When the melt temperature is 730-760° C., the Mg-Zn melt is subjected to primary inert gas rotary blowing refining to obtain a purified Mg-Zn melt;
[0009] When the melt temperature is 720-750° C., adding an erbium source and a ytterbium source to the purified Mg-Zn melt for melting to obtain a Mg-Zn-Er-Yb melt;
[0010] When the melt temperature is 680-720° C., the Mg-Zn-Er-Yb melt is subjected to secondary inert gas rotary blowing refining to obtain a purified Mg-Zn-Er-Yb melt;
[0011] adding a lithium source to the purified Mg-Zn-Er-Yb melt and melting the melt to obtain a Mg-Zn-Er-Yb-Li melt;
[0012] When the melt temperature is 660-720° C., a refining flux is used to perform three-stage flux refining on the Mg-Zn-Er-Yb-Li melt.
[0013] Preferably, the conditions for the primary inert gas rotary blowing refining include: nozzle rotation speed of 100-300 r / min, inert gas flow rate of 1-5 L / min, and blowing time of 2-10 min.
[0014] Preferably, the conditions for the secondary inert gas rotary blowing refining include: nozzle speed of 50-350 r / min, inert gas flow rate of 1-5 L / min, and blowing time of 3-15 min.
[0015] Preferably, the refining flux comprises the following components in percentage by mass: 25-55% sodium bromide, 10-35% calcium chloride, 10-35% lithium chloride, 5-25% lithium fluoride, 1-8% erbium chloride, 1-8% ytterbium chloride, and 5-15% carbonate foaming agent.
[0016] Preferably, the amount of the refining flux added is 1-6% of the mass of the Mg-Zn-Er-Yb-Li melt.
[0017] Preferably, the carbonate foaming agent is one or more of lithium carbonate, magnesium carbonate, zinc carbonate, erbium carbonate and ytterbium carbonate.
[0018] Preferably, the Mg-Li-Zn-Er-Yb alloy comprises the following elemental composition in percentage by mass: Li 6-14%, Zn 2-10%, Er 0.2-2%, Yb 0.2-2%, and the balance is Mg.
[0019] Preferably, the tertiary refining time is 5 to 10 minutes, and the insulation temperature is 660 to 720°C.
[0020] Preferably, when the lithium source is added, the temperature of the purified Mg-Zn-Er-Yb melt is 660-720°C.
[0021] Preferably, the magnesium source, zinc source, erbium source and ytterbium source are preheated before melting, and the preheating temperature is 180-200°C.
[0022] The invention provides a smelting and purification method of a Mg-Li-Zn-Er-Yb alloy for three-dimensional printing, comprising the following steps: according to the composition of the Mg-Li-Zn-Er-Yb alloy, a magnesium source is melted to obtain a magnesium melt, and a zinc source is added to melt the magnesium melt when the temperature of the magnesium melt is 680-700°C to obtain a Mg-Zn melt; when the melt temperature is 730-760°C, the Mg-Zn melt is subjected to primary inert gas rotary blowing refining to obtain a purified Mg-Zn melt; when the melt temperature is 720-750°C, a zinc source is added to the purified Mg-Zn melt to obtain a purified Mg-Zn melt; n melt is added with erbium source and ytterbium source to melt to obtain Mg-Zn-Er-Yb melt; when the melt temperature is 680-720°C, the Mg-Zn-Er-Yb melt is subjected to secondary inert gas rotary blowing refining to obtain purified Mg-Zn-Er-Yb melt; a lithium source is added to the purified Mg-Zn-Er-Yb melt to melt to obtain Mg-Zn-Er-Yb-Li melt; when the melt temperature is 660-720°C, the Mg-Zn-Er-Yb-Li melt is subjected to tertiary flux refining using a refining flux. In the method provided by the present invention, during the smelting process of the main elements Mg and Zn of the magnesium-lithium alloy, the melt temperature is about 730-760°C before the Er element and the Yb element are added, at which time some inclusions are easy to remove, and a first-level inert gas rotary blowing refining purification is performed at this temperature to reduce the slag content inside the melt for the first time; after the first-level refining is completed, an erbium source and a ytterbium source are added, and the heat preservation time is long, and there will be further oxidation to form new inclusions, so a second-level inert gas rotary blowing refining is performed in a temperature range of 680-720°C before the active element Li is added to further improve the purity of the melt and reduce the slag content; after the Li element is added at 660-720°C, the melt is in a state of being easily oxidized, and a third-level flux refining is performed at this time to further reduce the slag content inside the melt and ensure the purity of the melt before casting.
[0023] Furthermore, in the third-level flux refining of the present invention, the refining flux used includes the following components in percentage by mass: 25-55% sodium bromide, 10-35% calcium chloride, 10-35% lithium chloride, 5-25% lithium fluoride, 1-8% erbium chloride, 1-8% ytterbium chloride, and 5-15% carbonate foaming agent. The refining flux can reduce the Li burn-out rate and the Er and Yb sedimentation rates, does not react with lithium elements during use, can reduce lithium losses, and ensure the lithium element recovery rate; the refining flux also has an adsorption effect, wherein the carbonate foaming agent is thermally decomposed to continuously release tiny inert gas bubbles, which will adsorb non-metallic inclusions during the floating process, causing them to agglomerate into large particles, greatly improving the removal rate of various inclusions, and the refining effect is stable, and it is easy to separate from the alloy liquid for convenient slag removal.
[0024] Moreover, the refining flux used in the present invention has a better melting point, density and wettability, and has the functions of a refining agent and a covering agent. When used as a covering agent, it can effectively isolate the air and provide sufficient protection for the melt. At the same time, the released protective gas dilutes harmful gases such as hydrogen chloride, significantly reducing the emission of harmful gases during the smelting process, achieving the purpose of being pollution-free; when used as a refining agent, it can fully contact with inclusions in the melt to remove the inclusions and ensure the refining effect; and the present invention uses the refining flux to reduce the amount of the flux.
[0025] The slag content of the magnesium-lithium alloy obtained by the method provided by the present invention is greatly reduced, the burn-out rate of the Li element is reduced, the sedimentation rates of the Er element and the Yb element are reduced, and the mechanical properties are improved, providing technical support for the development of high-quality magnesium-lithium alloys and three-dimensional printing applications; and the smelting cost is reduced. DETAILED DESCRIPTION
[0026] The present invention provides a smelting and purification method of a Mg-Li-Zn-Er-Yb alloy for three-dimensional printing, comprising the following steps:
[0027] According to the composition of the Mg-Li-Zn-Er-Yb alloy, a magnesium source is melted to obtain a magnesium melt, and a zinc source is added and melted when the temperature of the magnesium melt is 680-700° C. to obtain a Mg-Zn melt;
[0028] When the melt temperature is 730-760° C., the Mg-Zn melt is subjected to primary inert gas rotary blowing refining to obtain a purified Mg-Zn melt;
[0029] When the melt temperature is 720-750° C., adding an erbium source and a ytterbium source to the purified Mg-Zn melt for melting to obtain a Mg-Zn-Er-Yb melt;
[0030] When the melt temperature is 680-720° C., the Mg-Zn-Er-Yb melt is subjected to secondary inert gas rotary blowing refining to obtain a purified Mg-Zn-Er-Yb melt;
[0031] adding a lithium source to the purified Mg-Zn-Er-Yb melt and melting the melt to obtain a Mg-Zn-Er-Yb-Li melt;
[0032] When the melt temperature is 660-720° C., a refining flux is used to perform three-stage flux refining on the Mg-Zn-Er-Yb-Li melt.
[0033] In the method provided by the present invention, the melt temperature is about 730-760°C before the Er source and the ytterbium source are added. At this time, some inclusions are easy to remove. At this temperature, the first-level inert gas rotary blowing refining is carried out to reduce the slag content inside the melt for the first time. After the first-level inert gas rotary blowing refining is completed, the erbium source and the ytterbium source will be added. The heat preservation time is long, and there will be further oxidation phenomenon to form new inclusions. Therefore, the temperature range is 680-720°C. Before adding the active element Li, the second-level inert gas rotary blowing refining is carried out to further improve the purity of the melt and reduce the slag content. After the Li element is added at 660-720°C, the melt is in a state of being extremely easy to oxidize. At this time, the third-level flux refining is carried out to reduce the Li burn-out rate and the Er and Yb sedimentation rates, and the slag content inside the melt can be further reduced to ensure the purity of the melt before casting.
[0034] The present invention melts the magnesium source according to the composition of the Mg-Li-Zn-Er-Yb alloy to obtain a magnesium melt. The present invention has no special restrictions on the method of melting the magnesium source, and a technical solution for melting the magnesium source well known to those skilled in the art can be used;
[0035] After obtaining the magnesium melt, the present invention adds a zinc source to melt when the temperature of the magnesium melt is 680-700°C to obtain a Mg-Zn melt. In the present invention, the temperature of the magnesium melt may be specifically 680, 690 or 700°C. In an embodiment of the present invention, the Mg-Li-Zn-Er-Yb alloy preferably includes the following elemental composition in mass percentage: Li 6-14%, Zn 2-10%, Er 0.2-2%, Yb 0.2-2%, and the balance is Mg.
[0036] In the present invention, the Mg-Li-Zn-Er-Yb alloy preferably includes Li 6-14wt%, and in specific embodiments may be 6, 7, 8, 9, 10, 11, 12, 13 or 14wt%.
[0037] In the present invention, the Mg-Li-Zn-Er-Yb alloy preferably includes 2-10 wt % Zn, and in specific embodiments may be 2, 3, 4, 5, 6, 7, 8, 9 or 10 wt %.
[0038] In the present invention, the Mg-Li-Zn-Er-Yb alloy preferably includes Er 0.2~2wt%, and in specific embodiments it can be 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 2wt%.
[0039] In the present invention, the Mg-Li-Zn-Er-Yb alloy preferably includes 0.2-2wt% Yb, and in specific embodiments may be 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 2wt%.
[0040] In the present invention, the Mg—Li—Zn—Er—Yb alloy preferably includes a balance of Mg.
[0041] The present invention has no particular limitation on the types of the magnesium source and the zinc source, and any type of magnesium source and zinc source known to those skilled in the art may be used. In an embodiment of the present invention, the magnesium source may be pure magnesium, and the zinc source may be pure zinc.
[0042] In the present invention, the magnesium source and the zinc source are preferably preheated before melting, and the preheating temperature is preferably 180-200°C, and in specific embodiments may be specifically 180, 190 or 200°C.
[0043] The present invention has no special limitation on the melting method, and the technical solution for melting magnesium-lithium alloys well known to those skilled in the art can be adopted.
[0044] After obtaining the Mg-Zn melt, the present invention performs a primary inert gas rotary blowing refining on the Mg-Zn melt when the melt temperature is 730-760° C. to obtain a purified Mg-Zn melt. In an embodiment of the present invention, the primary inert gas rotary blowing refining is performed using an inert gas rotary blowing device, and the present invention has no particular limitation on the model of the inert gas rotary blowing device. In the present invention, the inert gas can specifically be helium or argon. In the present invention, the nozzle speed during the first-level inert gas rotary blowing refining is preferably 100-300r / min, and in the embodiment, it can be specifically 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290 or 300r / min; the inert gas flow rate during the first-level inert gas rotary blowing refining is preferably 1-5L / min, and in the embodiment, it can be specifically 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5 or 5L / min; the blowing time during the first-level inert gas rotary blowing refining is preferably 2-10min, and in the embodiment, it can be specifically 2, 3, 4, 5, 6, 7, 8, 9 or 10min.
[0045] In an embodiment of the present invention, the temperature of the melt during the primary inert gas rotary blowing refining may specifically be 730, 735, 740, 745, 750, 755 or 760°C.
[0046] After obtaining the purified Mg-Zn melt, the present invention adds an erbium source and a ytterbium source to the purified Mg-Zn melt for melting to obtain a Mg-Zn-Er-Yb melt. The present invention preferably adds an erbium source and a ytterbium source to melt when the melt temperature is 720-750°C after the primary inert gas rotary blowing refining, which may be specifically 720, 730, 740 or 750°C in the embodiment, and keeps the temperature at the specified temperature for 5-10 minutes after adding the erbium source and the ytterbium source. The present invention has no special restrictions on the types of the erbium source and the ytterbium source, and the erbium source and the ytterbium source well known to those skilled in the art can be used, such as magnesium erbium master alloy and magnesium ytterbium master alloy. In the present invention, the erbium source and the ytterbium source are preferably preheated before melting, and the preheating temperature is preferably 180-200°C, which may be specifically 180, 190 or 200°C.
[0047] After obtaining the Mg-Zn-Er-Yb melt, the present invention performs secondary inert gas rotary blowing refining on the Mg-Zn-Er-Yb melt when the melt temperature is 680-720°C to obtain a purified Mg-Zn-Er-Yb melt. In an embodiment of the present invention, the secondary inert gas rotary blowing refining is performed using an inert gas rotary blowing device, and the present invention has no special restrictions on the model of the inert gas rotary blowing device. In the present invention, the inert gas can specifically be helium or argon. In the present invention, the nozzle speed during the secondary inert gas rotary blowing refining is preferably 50-350r / min, and in the embodiments, it can be specifically 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300, 310, 320, 330, 340 or 350r / min; the inert gas flow rate during the secondary inert gas rotary blowing refining is preferably 1-5L / min, and in the embodiments it can be specifically 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5 or 5L / min; the secondary inert gas rotary blowing refining time is preferably 3-15min, and in the embodiments it can be specifically 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15min.
[0048] In an embodiment of the present invention, the temperature of the melt during the secondary inert gas rotary blowing refining may specifically be 680, 690, 700, 710 or 720°C.
[0049] After the secondary inert gas rotary blowing refining, the present invention adds a lithium source to the purified Mg-Zn-Er-Yb melt for melting to obtain a Mg-Zn-Er-Yb-Li melt. The present invention has no special restrictions on the type of the lithium source, and a lithium source familiar to those skilled in the art can be used, such as pure lithium. In an embodiment of the present invention, a lithium cover is preferably used to press pure lithium into 2 / 3 below the melt surface to completely melt it. After the secondary inert gas rotary blowing refining, the present invention preferably adds a lithium source for melting when the melt temperature is 660~720℃, which can be specifically 660, 670, 680, 690, 700, 710 or 720℃ in the embodiment.
[0050] After obtaining the Mg-Zn-Er-Yb-Li melt, the present invention uses a refining flux to perform three-stage flux refining on the Mg-Zn-Er-Yb-Li melt when the melt temperature is 660-720° C. In an embodiment of the present invention, the temperature of the melt during the three-stage flux refining can be specifically 660, 670, 680, 690, 700, 710 or 720° C.
[0051] In the present invention, the refining flux comprises the following components in percentage by mass: 25-55% sodium bromide, 10-35% calcium chloride, 10-35% lithium chloride, 5-25% lithium fluoride, 1-8% erbium chloride, 1-8% ytterbium chloride, and 5-15% carbonate foaming agent.
[0052] In the present invention, the refining flux comprises 25-55 wt% of sodium bromide, which may be 25, 30, 35, 37, 40, 45, 50 or 55 wt% in the embodiment. In the present invention, the sodium bromide acts as a thickener to increase the viscosity of the liquid flux.
[0053] In the present invention, the refining flux includes 10-35wt% of calcium chloride, which may be 10, 15, 19, 20, 25, 30 or 35wt% in the embodiment. In the present invention, the role of the calcium chloride is to increase the viscosity of the flux, act as a thickener, and enable the slag to aggregate.
[0054] In the present invention, the refining flux includes 10-35wt% of lithium chloride, which may be 10, 15, 20, 25, 30 or 35wt% in the embodiment. In the present invention, the lithium chloride is used to wet the melt and aggregate the inclusions.
[0055] In the present invention, the refining flux includes 5-25wt% lithium fluoride, which may be 5, 9, 10, 15, 16, 20 or 25wt% in the embodiment. In the present invention, the lithium fluoride is used to wet the melt and aggregate the inclusions.
[0056] In the present invention, the refining flux includes 1-8 wt % of erbium chloride, and in embodiments, it may be specifically 1, 2, 3, 4, 5, 6, 7 or 8 wt %.
[0057] In the present invention, the refining flux includes 1-8wt% of ytterbium chloride, and in embodiments, it may be specifically 1, 2, 3, 4, 5, 6, 7 or 8wt%.
[0058] In the present invention, the refining flux includes 5-15wt% of a carbonate foaming agent, which may be 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15wt% in the embodiment. In the present invention, the carbonate foaming agent is preferably one or more of lithium carbonate, magnesium carbonate, zinc carbonate, erbium carbonate and ytterbium carbonate, which may be one or two; when there are two, ytterbium carbonate and erbium carbonate are preferred, and the mass ratio of ytterbium carbonate to erbium carbonate is preferably 1:2; zinc carbonate and lithium carbonate may also be used, and the mass ratio of zinc carbonate to lithium carbonate is preferably 1:1.
[0059] In the present invention, erbium chloride can compensate for the burning loss of erbium elements, ytterbium chloride can compensate for the burning loss of ytterbium elements, and lithium chloride and lithium fluoride can compensate for the burning loss of lithium elements, thereby improving the composition stability of the prepared magnesium-lithium alloy. Under high temperature conditions, the carbonate foaming agent is thermally decomposed to produce carbon dioxide gas to form bubbles. On the one hand, these bubbles make the covering flux float on the surface of the melt and will not sink into the melt, which can maintain the covering and protection effects for a long time and reduce the amount of flux used; on the other hand, these bubbles react with magnesium and cover the surface of the melt, which also has the effect of preventing the melt from oxidative burning.
[0060] In the present invention, the addition amount of the refining flux is preferably 1-6% of the mass of the Mg-Zn-Er-Yb-Li melt, and may be specifically 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5 or 6%.
[0061] In the present invention, the time of the tertiary flux refining is preferably 5 to 10 minutes, specifically 5, 6, 7, 8, 9 or 10 minutes; the insulation temperature is preferably 660°C to 720°C, specifically 660, 670, 680, 690, 700, 710 or 720°C.
[0062] After the three-stage flux refining, the present invention preferably casts the obtained purified Mg-Zn-Er-Yb-Li melt to obtain an alloy ingot; and performs a solid solution treatment on the alloy ingot and then water quenches it to obtain a T4 state magnesium-lithium alloy.
[0063] After the three-stage refining, the present invention preferably controls the temperature of the purified Mg-Zn-Er-Yb-Li melt to 680-720°C, which can be specifically 680, 690, 700, 710 or 720°C, removes the surface covering solvent, and casts the obtained purified Mg-Zn-Er-Yb-Li melt to obtain an alloy ingot. The present invention has no special restrictions on the casting mold, which can be a steel mold in the embodiment of the present invention. In the present invention, the mold is preferably preheated, and the preheating temperature can be specifically 200°C.
[0064] After obtaining the alloy ingot, the present invention performs a solution treatment on the alloy ingot and then water quenches it to obtain a T4 state magnesium-lithium alloy. In the present invention, the temperature of the solution treatment is preferably 300 to 350° C.; the holding time of the solution treatment is preferably 2 to 6 hours. The present invention has no special restrictions on the water quenching method, and the water quenching technical solution familiar to those skilled in the art can be used.
[0065] It should be noted that the following embodiments and features in the embodiments may be combined with each other in the absence of conflict; and, based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in the field without making any creative work are within the scope of protection of the present disclosure.
[0066] It should be noted that various aspects of the embodiments within the scope of the appended claims are described below. It should be apparent that the aspects described herein may be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present disclosure, it should be understood by those skilled in the art that an aspect described herein may be implemented independently of any other aspect, and two or more of these aspects may be combined in various ways. For example, any number of aspects described herein may be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein may be used to implement this device and / or practice this method.
[0067] Example 1
[0068] According to the composition and weight percentage of Li 6%, Zn 2%, Er 0.2%, Yb 0.2%, and the balance magnesium alloy, pure magnesium, pure zinc, magnesium-erbium master alloy and magnesium-ytterbium master alloy are prepared, the magnesium source is first melted, and then the zinc source is added and melted at a melt temperature of 700° C. to obtain a Mg-Zn melt;
[0069] Before adding the magnesium-erbium master alloy and the magnesium-ytterbium master alloy, at a temperature of 760°C, the obtained Mg-Zn melt was subjected to a first-stage argon rotary blowing refining by using an argon rotary blowing device: the nozzle speed was 300 r / min, the gas flow rate was 1 L / min, and the blowing time was 10 min;
[0070] After the first-stage argon rotary injection refining, the preheated magnesium-erbium master alloy and magnesium-ytterbium master alloy are added and melted at 740°C to obtain a Mg-Zn-Er-Yb melt;
[0071] Before adding Li element, at the temperature of 720°C, Mg-Zn-Er-Yb melt was subjected to secondary argon rotary blowing refining by using argon rotary blowing equipment: nozzle speed 100r / min, gas flow rate 5L / min, blowing time 3min;
[0072] At 700°C, pure lithium is pressed into the melt 2 / 3 below the liquid surface by a lithium cover to completely melt it, and a Mg-Zn-Er-Yb-Li melt is obtained. When the temperature is 720°C, the Mg-Zn-Er-Yb-Li melt is subjected to three-stage flux refining by a refining flux for 5 minutes. The amount of refining flux added is 1% of the mass of the Mg-Zn-Er-Yb-Li melt. The composition of the refining flux is: 25wt% sodium bromide, 35wt% calcium chloride, 20wt% lithium chloride, 5wt% lithium fluoride, 1wt% erbium chloride, 1% ytterbium chloride and, 13wt% lithium carbonate;
[0073] After refining, the temperature is controlled at 720°C, the flux covering the surface of the melt is removed, and the melt is cast into a steel mold preheated to about 200°C to obtain a Mg-6Li-2Zn-0.2Er-0.2Yb alloy ingot.
[0074] The obtained Mg-6Li-2Zn-0.2Er-0.2Yb alloy ingot was solution treated at 300°C for 6h and finally water quenched to obtain T4 state magnesium-lithium alloy.
[0075] The present invention performs chemical composition analysis on the obtained T4 state magnesium-lithium alloy, and the results are shown in Table 1.
[0076] Table 1 Chemical element composition of T4 magnesium-lithium alloy obtained in Example 1 (wt%)
[0077]
[0078] Example 2
[0079] The alloy is prepared according to the composition and weight percentage of Li 14%, Zn 10%, Er 2%, Yb 2% and the balance of magnesium, pure magnesium, pure zinc, magnesium-erbium master alloy and magnesium-ytterbium master alloy are preheated to 180° C., the magnesium source is first melted, and then the zinc source is added and melted at a melt temperature of 700° C. to obtain a Mg-Zn melt;
[0080] Before adding the magnesium-erbium master alloy and the magnesium-ytterbium master alloy, at a temperature of 730°C, the obtained Mg-Zn melt was subjected to a first-stage argon rotary blowing refining using an argon rotary blowing device: the nozzle speed was 100 r / min, the gas flow rate was 5 L / min, and the blowing time was 2 min;
[0081] After the first-stage argon rotary injection refining, the preheated magnesium-erbium master alloy and magnesium-ytterbium master alloy are added and melted at 700°C to obtain a Mg-Zn-Er-Yb melt;
[0082] Before adding Li element, at the temperature of 680°C, Mg-Zn-Er-Yb melt was subjected to secondary argon rotary blowing refining by using argon rotary blowing equipment: nozzle speed 100r / min, gas flow rate 5L / min, blowing time 2min;
[0083] At 660°C, pure lithium is pressed into the melt 2 / 3 below the liquid surface by a lithium cover to completely melt it, and a Mg-Zn-Er-Yb-Li melt is obtained. When the temperature is 660°C, the Mg-Zn-Er-Yb-Li melt is subjected to three-stage flux refining by a refining flux for 10 minutes. The amount of refining flux added is 6% of the mass of the Mg-Zn-Er-Yb-Li melt. The composition of the refining flux is: 55wt% sodium bromide, 10wt% calcium chloride, 10wt% lithium chloride, 5wt% lithium fluoride, 7wt% erbium chloride, 8% ytterbium chloride, and 5wt% zinc carbonate;
[0084] After refining, the temperature is controlled at 680°C, the flux covering the surface of the melt is removed, and the melt is cast into a steel mold preheated to about 200°C to obtain a Mg-14Li-10Zn-2Er-2Yb alloy ingot.
[0085] The obtained Mg-14Li-10Zn-2Er-2Yb alloy ingot was kept at 300°C for 6 hours for solution treatment, and finally water quenched to obtain T4 state magnesium-lithium alloy.
[0086] The present invention performs chemical composition analysis on the obtained T4 state magnesium-lithium alloy, and the results are shown in Table 2.
[0087] Table 2 Chemical element composition of T4 magnesium-lithium alloy obtained in Example 2 (wt%)
[0088]
[0089] Example 3
[0090] Preheating pure magnesium, pure zinc, magnesium-erbium master alloy and magnesium-ytterbium master alloy to 190° C., melting the preheated pure magnesium and pure zinc in a crucible to obtain a Mg-Zn melt;
[0091] Before adding the magnesium-erbium master alloy and the magnesium-ytterbium master alloy, at a temperature of 745°C, the obtained Mg-Zn melt was subjected to a first-stage argon rotary blowing refining using an argon rotary blowing device: the nozzle speed was 200 r / min, the gas flow rate was 3 L / min, and the blowing time was 6 min;
[0092] After the first-stage argon rotary injection refining, the preheated magnesium-erbium master alloy and magnesium-ytterbium master alloy are added and melted at 720°C to obtain a Mg-Zn-Er-Yb melt;
[0093] Before adding Li element, at the temperature of 700°C, the Mg-Zn-Er-Yb melt was subjected to secondary argon rotary blowing refining using argon rotary blowing equipment: nozzle speed 200r / min, gas flow rate 3L / min, blowing time 9min;
[0094] At 680°C, pure lithium is pressed into the melt 2 / 3 below the liquid surface by a lithium cover to completely melt it, and a Mg-Zn-Er-Yb-Li melt is obtained. When the temperature is 690°C, the Mg-Zn-Er-Yb-Li melt is subjected to three-stage flux refining by a refining flux for 8 minutes. The amount of refining flux added is 3.5% of the mass of the Mg-Zn-Er-Yb-Li melt. The composition of the refining flux is: 37wt% sodium bromide, 20wt% calcium chloride, 15wt% lithium chloride, 10wt% lithium fluoride, 5wt% erbium chloride, 8% ytterbium chloride, 5wt% ytterbium carbonate and erbium carbonate (the mass ratio of the two is 1:2);
[0095] After refining, the temperature is controlled at 700°C, the flux covering the surface of the melt is removed, and the melt is cast into a steel mold preheated to about 200°C to obtain a Mg-8Li-5Zn-0.5Er-0.5Yb alloy ingot.
[0096] The obtained Mg-8Li-5Zn-0.5Er-0.5Yb alloy ingot was kept at 350°C for 4 hours for solution treatment, and finally quenched in water to obtain T4 state magnesium-lithium alloy.
[0097] The present invention performs chemical composition analysis on the obtained T4 state magnesium-lithium alloy, and the results are shown in Table 3.
[0098] Table 3 Chemical element composition of T4 magnesium-lithium alloy obtained in Example 3 (wt%)
[0099]
[0100] Example 4
[0101] The alloy is prepared according to the composition and weight percentage of Li 10%, Zn 6%, Er 1%, Yb 1% and the balance of magnesium, pure magnesium, pure zinc, magnesium-erbium master alloy and magnesium-ytterbium master alloy are preheated to 200° C., the magnesium source is first melted, and then the zinc source is added and melted at a melt temperature of 700° C. to obtain a Mg-Zn melt;
[0102] Before adding the magnesium-erbium master alloy and the magnesium-ytterbium master alloy, at a temperature of 740°C, the obtained Mg-Zn melt was subjected to a first-stage argon rotary blowing refining using an argon rotary blowing device: the nozzle speed was 300 r / min, the gas flow rate was 3 L / min, and the blowing time was 6 min;
[0103] After the first-stage argon rotary injection refining, the preheated magnesium-erbium master alloy and magnesium-ytterbium master alloy are added and melted at 710°C to obtain a Mg-Zn-Er-Yb melt;
[0104] Before adding Li element, at the temperature of 690°C, the obtained Mg-Zn-Er-Yb melt was subjected to secondary argon rotary blowing refining by using argon rotary blowing equipment: nozzle speed 200r / min, gas flow rate 3L / min, blowing time 15min;
[0105] At 670℃, pure lithium is pressed into 2 / 3 of the melt surface by a lithium cover to completely melt it, and a Mg-Zn-Er-Yb-Li melt is obtained. When the temperature is 690℃, the Mg-Zn-Er-Yb-Li melt is subjected to three-stage flux refining by a refining flux for 8 minutes. The amount of refining flux added is 2% of the mass of the Mg-Zn-Er-Yb-Li melt. The composition of the refining flux is: 45wt% sodium bromide, 15wt% calcium chloride, 10wt% lithium chloride, 9wt% lithium fluoride, 6wt% erbium chloride, 8% ytterbium chloride, 7wt% lithium carbonate and zinc carbonate (the mass ratio of the two is 1:1);
[0106] After refining, the temperature is controlled at 700°C, the flux covering the surface of the melt is removed, and the melt is cast into a steel mold preheated to about 200°C to obtain a Mg-10Li-6Zn-1Er-1Yb alloy ingot.
[0107] The obtained Mg-10Li-6Zn-1Er-1Yb alloy ingot was kept at 325°C for 5 hours for solution treatment, and finally quenched in water to obtain T4 state magnesium-lithium alloy.
[0108] The present invention performs chemical composition analysis on the obtained T4 state magnesium-lithium alloy, and the results are shown in Table 4.
[0109] Table 4 Chemical element composition of T4 magnesium-lithium alloy obtained in Example 4 (wt%)
[0110]
[0111] Example 5
[0112] According to the composition and weight percentage of the alloy of Li 9%, Zn 6%, Er 1%, Yb 0.5% and the balance of magnesium, pure magnesium, pure zinc, magnesium-erbium master alloy and magnesium-ytterbium master alloy are preheated to 180° C., the magnesium source is first melted, and then the zinc source is added and melted at a melt temperature of 700° C. to obtain a Mg-Zn melt;
[0113] Before adding the magnesium-erbium master alloy and the magnesium-ytterbium master alloy, at a temperature of 750°C, the obtained Mg-Zn melt was subjected to a first-stage argon rotary blowing refining using an argon rotary blowing device: the nozzle speed was 200 r / min, the gas flow rate was 3 L / min, and the blowing time was 6 min;
[0114] After the first-stage argon rotary injection refining, the preheated magnesium-erbium master alloy and magnesium-ytterbium master alloy are added and melted at 720°C to obtain a Mg-Zn-Er-Yb melt;
[0115] Before adding Li element, at the temperature of 680°C, the obtained Mg-Zn-Er-Yb melt was subjected to secondary argon rotary blowing refining by using argon rotary blowing equipment: nozzle speed 200r / min, gas flow rate 3L / min, blowing time 10min;
[0116] At 670°C, pure lithium is pressed into the melt 2 / 3 below the liquid surface by a lithium cover to completely melt it, and a Mg-Zn-Er-Yb-Li melt is obtained. When the temperature is 690°C, the Mg-Zn-Er-Yb-Li melt is subjected to three-stage flux refining by a refining flux for 8 minutes. The amount of refining flux added is 3% of the mass of the Mg-Zn-Er-Yb-Li melt. The composition of the refining flux is: 50wt% sodium bromide, 10wt% calcium chloride, 12wt% lithium chloride, 16wt% lithium fluoride, 2wt% erbium chloride, 5% ytterbium chloride, and 5% lithium carbonate;
[0117] After refining, the temperature was controlled at 690°C and the melt was cast into a steel mold preheated to about 200°C to obtain a Mg-9Li-6Zn-1Er-0.5Yb alloy ingot.
[0118] The obtained Mg-9Li-6Zn-1Er-0.5Yb alloy ingot was kept at 300°C for 6 hours for solution treatment, and finally water quenched to obtain T4 state magnesium-lithium alloy.
[0119] The present invention performs chemical composition analysis on the obtained T4 state magnesium-lithium alloy, and the results are shown in Table 5.
[0120] Table 5 Chemical element composition of T4 magnesium-lithium alloy obtained in Example 5 (wt%)
[0121]
[0122] Comparative Example 1
[0123] The alloy is prepared according to the composition and weight percentage of Li 8%, Zn 5%, Er 0.5%, Yb 0.5% and the balance of magnesium, and pure magnesium, pure zinc, magnesium-erbium master alloy and magnesium-ytterbium master alloy are preheated to 200° C., the magnesium source is first melted, and then pure zinc is added to melt at a melt temperature of 700° C., and then magnesium-erbium master alloy and magnesium-ytterbium master alloy are added to melt at a melt temperature of 730° C. to obtain a Mg-Zn-Er-Yb melt;
[0124] At 680°C, pure lithium was pressed into the melt 2 / 3 below the liquid surface by a lithium cover to make it completely melted. After the addition of Li element, at the temperature of 680°C, the obtained Mg-Zn-Er-Yb-Li melt was subjected to primary argon rotary blowing refining by using argon rotary blowing equipment: nozzle speed 200r / min, gas flow 3L / min, blowing time 6min;
[0125] After refining, the temperature was controlled at 700°C, and the melt was cast into a steel mold preheated to about 200°C to obtain a Mg-8Li-5Zn-0.5Er-0.5Yb alloy ingot;
[0126] The obtained Mg-8Li-5Zn-0.5Er-0.5Yb alloy ingot was kept at 350°C for 2 hours for solution treatment, and finally quenched in water to obtain T4 state magnesium-lithium alloy.
[0127] The present invention performs chemical composition analysis on the obtained T4 magnesium-lithium alloy, and the results are shown in Table 6.
[0128] Table 6 Chemical element composition of T4 magnesium-lithium alloy obtained in Comparative Example 1 (wt%)
[0129]
[0130] Comparative Example 2
[0131] According to the composition and weight percentage of the alloy of Li 8%, Zn 5%, Er 0.5%, Yb 0.5% and the balance of magnesium, pure magnesium, pure zinc, magnesium-erbium master alloy and magnesium-ytterbium master alloy are preheated to 200° C., the magnesium source is first melted, and then pure zinc is added to melt at a melt temperature of 700° C. to obtain a Mg-Zn melt;
[0132] Before adding the magnesium-erbium master alloy and the magnesium-ytterbium master alloy, at a temperature of 730°C, the obtained Mg-Zn melt was subjected to a first-stage argon rotary blowing refining using an argon rotary blowing device: the nozzle speed was 100 r / min, the gas flow rate was 5 L / min, and the blowing time was 2 min;
[0133] After the first-stage argon rotary injection refining, magnesium-erbium master alloy and magnesium-ytterbium master alloy are added and melted at 700°C to obtain Mg-Zn-Er-Yb melt;
[0134] At 680℃, pure lithium was pressed into the melt 2 / 3 below the liquid surface by a lithium cover to completely melt it. After adding the Li element, the Mg-Zn-Er-Yb-Li melt was subjected to secondary refining by an argon rotary blowing device at a temperature of 680℃: the nozzle speed was 100r / min, the gas flow rate was 5L / min, and the blowing time was 2min. After the refining was completed, the temperature was controlled at 700℃, and the melt was cast into a steel mold preheated to about 200℃ to obtain a Mg-8Li-5Zn-0.5Er-0.5Yb alloy ingot.
[0135] The obtained Mg-8Li-5Zn-0.5Er-0.5Yb alloy ingot was kept at 350°C for 2 hours for solution treatment, and finally quenched in water to obtain T4 state magnesium-lithium alloy.
[0136] The present invention performs chemical composition analysis on the obtained T4 state magnesium-lithium alloy, and the results are shown in Table 7.
[0137] Table 7 Chemical element composition of T4 magnesium-lithium alloy obtained in Comparative Example 2 (wt%)
[0138]
[0139] Comparative Example 3
[0140] The alloy is prepared according to the composition and weight percentage of Li 8%, Zn 5%, Er 0.5%, Yb 0.5% and the balance of magnesium, and pure magnesium, pure zinc, magnesium-erbium master alloy and magnesium-ytterbium master alloy are preheated to 200° C., the magnesium source is first melted, and then pure zinc is added to melt at a melt temperature of 700° C., and then magnesium-erbium master alloy and magnesium-ytterbium master alloy are added to melt at a melt temperature of 730° C. to obtain a Mg-Zn-Er-Yb melt;
[0141] At 680℃, pure lithium is pressed into the melt 2 / 3 below the liquid surface by a lithium cover to make it completely melted. After adding the Li element, the temperature is 690℃, and the refining flux is used for refining. The amount of refining flux added is 3.5% of the mass of the Mg-Zn-Er-Yb-Li melt. The composition of the refining flux is: 37wt% sodium bromide, 20wt% calcium chloride, 15wt% lithium chloride, 10wt% lithium fluoride, 5wt% erbium chloride, 8% ytterbium chloride, 5wt% ytterbium carbonate and erbium carbonate;
[0142] After refining, the temperature was controlled at 700°C, and the melt was cast into a steel mold preheated to about 200°C to obtain a Mg-8Li-5Zn-0.5Er-0.5Yb alloy ingot.
[0143] The obtained Mg-8Li-5Zn-0.5Er-0.5Yb alloy ingot was kept at 350°C for 2 hours for solution treatment, and finally quenched in water to obtain T4 state magnesium-lithium alloy.
[0144] The present invention performs chemical composition analysis on the obtained T4 state magnesium-lithium alloy, and the results are shown in Table 8.
[0145] Table 8 Chemical element composition of T4 magnesium-lithium alloy obtained in Comparative Example 3 (wt%)
[0146]
[0147] Test Results
[0148] The present invention adopts the test method of GB / T228.1-2010 "Tensile test of metallic materials Part 1: Room temperature test method" to measure the room temperature mechanical properties of the solid solution Mg-Li-Zn-Er-Yb alloy obtained by solution treatment in the embodiment and the comparative example, and the results are shown in Table 9.
[0149] Table 9 Room temperature mechanical properties of solid solution Mg-Li-Zn-Er-Yb alloys of the present invention and comparative examples
[0150]
[0151] The present invention adopts the test method of GB / T 13748.15-2005 "Chemical Analysis Methods for Magnesium and Magnesium Alloys" to measure the slag content, element burnout rate and sedimentation rate of the T4 state magnesium-lithium alloy obtained in the embodiment and the comparative example. The results are shown in Table 10.
[0152] Table 10 Slag content, Li burnout rate, and Er and Yb sedimentation rates of T4 state magnesium-lithium alloys obtained in the examples of the present invention and the comparative examples
[0153]
[0154] It can be seen from the embodiments and comparative examples that the present invention can significantly reduce the burnout of precious elements Li, Er and Yb, greatly reduce the content of melt inclusions, effectively improve the quality of magnesium-lithium alloys, and reduce the production cost of magnesium-lithium alloys, which can promote the popularization and application of such materials.
[0155] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.
Claims
1. A method for smelting and purifying Mg-Li-Zn-Er-Yb alloy for three-dimensional printing, characterized in that: The following steps are involved: According to the composition of the Mg-Li-Zn-Er-Yb alloy, a magnesium source is melted to obtain a magnesium melt, and a zinc source is added to melt when the temperature of the magnesium melt is 680-690° C. to obtain a Mg-Zn melt; When the melt temperature is 730-760° C., the Mg-Zn melt is subjected to primary inert gas rotary blowing refining to obtain a purified Mg-Zn melt; When the melt temperature is 720-750° C., adding an erbium source and a ytterbium source to the purified Mg-Zn melt for melting to obtain a Mg-Zn-Er-Yb melt; When the melt temperature is 680-720° C., the Mg-Zn-Er-Yb melt is subjected to secondary inert gas rotary blowing refining to obtain a purified Mg-Zn-Er-Yb melt; adding a lithium source to the purified Mg-Zn-Er-Yb melt and melting the melt to obtain a Mg-Li-Zn-Er-Yb melt; When the melt temperature is 660-720° C., the Mg-Li-Zn-Er-Yb melt is subjected to three-stage flux refining by using a refining flux, wherein the refining flux is composed of the following components in percentage by weight: 25-55% sodium bromide, 10-35% calcium chloride, 10-35% lithium chloride, 5-25% lithium fluoride, 1-8% erbium chloride, 1-8% ytterbium chloride, and 5-15% carbonate foaming agent; The Mg-Li-Zn-Er-Yb alloy is composed of the following elements in percentage by mass: Li 6-14%, Zn 2-10%, Er 0.2-2%, Yb 0.2-2%, and the balance is Mg.
2. The smelting purification method according to claim 1, characterized in that: The conditions for the primary inert gas rotary blowing refining include: nozzle rotation speed of 100-300 r / min, inert gas flow rate of 1-5 L / min, and blowing time of 2-10 min.
3. The smelting purification method according to claim 1, characterized in that: The conditions for the secondary inert gas rotary blowing refining include: nozzle rotation speed of 50-350r / min, inert gas flow rate of 1-5L / min, and blowing time of 3-15min.
4. The smelting purification method according to claim 1, characterized in that: The amount of the refining flux added is 1-6% of the mass of the Mg-Li-Zn-Er-Yb melt.
5. The smelting purification method according to claim 1, characterized in that: The carbonate foaming agent is one or more of lithium carbonate, magnesium carbonate, zinc carbonate, erbium carbonate and ytterbium carbonate.
6. The smelting purification method according to claim 1, characterized in that: The refining time of the tertiary flux is 5 to 10 minutes, and the insulation temperature is 660 to 720°C.
7. The smelting purification method according to claim 1, characterized in that: When the lithium source is added, the temperature of the purified Mg-Zn-Er-Yb melt is 660-720°C.
8. The smelting purification method according to claim 1, characterized in that: The magnesium source, zinc source, erbium source and ytterbium source are preheated before melting, and the preheating temperature is 180-200°C.
Citation Information
Patent Citations
Er-containing high-strength magnesium lithium alloy and preparation method thereof
CN108315619A
Melt refining flux containing rare-earth magnesium lithium alloy, and preparation method thereof
CN108384974A
Preparation method for high-strength Mg-Li-Zn-Er ultra-light alloy
CN108842075A
Refining method for cast aluminum lithium alloy with high lithium content
CN108950264A
Continuous production method of high-quality multi-element rare earth magnesium alloy with controllable end-point components
CN113106275A