Montmorillonite carrier and preparation method thereof, preparation method of hydrodeoxygenation catalyst and application thereof

By acidizing the modified montmorillonite support, a high-activity and high-stability hydrodeoxygenation catalyst is formed, which solves the problems of low catalyst activity and poor stability in the prior art, and improves the specific hydrocarbons in biodiesel Yield and deoxygenation rate reduce costs.

CN116408056BActive Publication Date: 2024-11-22PETROCHINA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111681115.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-31
Publication Date
2024-11-22
Estimated Expiration
2041-12-31

AI Technical Summary

Technical Problem

The existing hydrodeoxygenation catalysts have problems such as low activity, poor stability, high cost and low deoxygenation rate in biodiesel preparation. Especially when using alumina as a support, the hydrothermal stability is poor, which affects the catalytic performance.

Method used

The acidified modified montmorillonite is used as a support to prepare a montmorillonite support through acidification and cross-linking reaction of acidifiers, and the support is supported with the active metals such as nickel and molybdenum to form a highly active and highly stable hydrodeoxygenation catalyst.

Benefits of technology

The activity and stability of the catalyst are improved, the yield and deoxygenation rates of pentane, hexadecane, heptadecane and octadecane in biodiesel are enhanced, the preparation cost is reduced, and the problem of poor hydrothermal stability is overcome.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a montmorillonite carrier and a preparation method thereof, a preparation method of a hydrodeoxygenation catalyst and an application thereof. The preparation method of the montmorillonite carrier comprises: acidifying and modifying the montmorillonite by an acidifying agent, then adding a crosslinking agent for crosslinking reaction, and calcining to obtain the montmorillonite carrier. The preparation method of the invention uses the acidified modified montmorillonite as a raw material to prepare the montmorillonite carrier. The preparation method has low cost, and the hydrodeoxygenation catalyst prepared from the montmorillonite carrier has the advantages of high activity, high stability, etc. The hydrodeoxygenation catalyst is improved in terms of stability, selectivity, and activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of biomass oil hydrodeoxygenation catalysts, and specifically relates to a carrier prepared with montmorillonite as a raw material and a preparation method thereof, a preparation method of a hydrodeoxygenation catalyst comprising the montmorillonite carrier and a non-precious metal, and an application thereof. Background Art

[0002] Montmorillonite is a natural mineral that can be used as a catalytic and adsorbent material. Especially after modification, it can obtain a porous structure material and has been widely used as an industrial catalyst, carrier and adsorbent.

[0003] As early as the 1930s, Hondry E found that acidified montmorillonite could obtain a higher gasoline yield when used as a petroleum cracking catalyst. This type of modified montmorillonite was widely used as a commercial catalyst until the mid-1960s when it was replaced by zeolite catalysts with better thermal stability and selectivity. However, due to its special properties, such as small dosage, reproducibility and recycling, easy preparation, mild reaction conditions, high yield and selectivity, it has good catalytic application prospects in establishing environmentally friendly technology. Commercial modified montmorillonite such as K-10 or KSF (products of Sud-Chemie or Fluka Chemical in Germany) and F-13 or F-20 (produced by Engelhard in the United States) are widely used in hydrocarbon processing in industry as acid catalysts or adsorbents. Among them, K-10 is the most studied acidified montmorillonite in business.

[0004] Clay or acidified clay is also a good carrier for many inorganic salt catalysts and other reagents. These compounds include Lewis acids (such as FeCl3, ZnCl2, and Fe(N03)3 or Cu(N03)2. The research results of Laszlo et al. show that after using montmorillonite to load FeCl3 and ZnCl2, the analysis found that its Lewis acid strength was significantly enhanced. It shows better catalytic performance in Friedel--Crafts reaction. Laszlo et al. believe that the active site appears on the edge of the clay platelet structure layer, and there is no proportional relationship with its surface area. Clark et al. used methanol Lewis acid reagent solution to immobilize on K-10 (acid-treated montmorillonite commercial product) by impregnation method, and after calcination and activation in air, a series of catalysts were formed. They showed good catalytic performance in Friedel--Crafts alkylation reaction, especially the catalyst loaded with ZnCl2 (known as Clayzic abroad) had high single selectivity and yield in the reaction.

[0005] As the consumption of fossil energy increases year by year and the reserves of fossil resources decrease year by year, the world will face an energy shortage crisis. At the same time, with the progress of society, people's living standards are gradually improving, and their awareness of environmental protection is also increasing. The development of new energy sources is imminent. Among them, biodiesel is one of the important and most promising clean fuels, which has attracted widespread attention at home and abroad.

[0006] Animal and plant oils are used as raw materials, which have a wide source and large quantity. However, they contain different numbers of carbon-carbon double bonds and a high oxygen content. In the process of preparing high-quality biodiesel, the core technology is the research on double bond saturation and hydrodeoxygenation catalysts. Albemarle Corporation in Holland patent, UOP LLC patent EP1728844A1, IFP patent CN101831315A, and Shanxi Coal Chemistry Research Institute of the Chinese Academy of Sciences patent CN1597859A all use alumina as a carrier and load one or more of nickel, cobalt, copper, iron, titanium, and lanthanum as active metals to prepare hydrodeoxygenation catalysts. The production process is relatively complicated and costly, with high pressure and hydrogen-to-oil ratio, high energy consumption, incomplete saturation of olefin double bonds and low deoxygenation rate. The catalyst activity is average and the stability needs to be improved.

[0007] Liang Wei, Li Baoshan and others published the effect of Mo additive on the structure and hydrodeoxygenation performance of silicon-pillared montmorillonite-supported nickel catalyst (Industrial Catalysis, June 2017; Vol. 25, No. 6) that silicon-pillared montmorillonite-supported bimetallic catalyst Mo-Ni / SPC was prepared by liquid phase reduction method using polyvinyl pyrrolidone as nanoparticle protective agent and hydrated hydrazine as reducing agent. The performance of Mo-Ni / SPC catalyst was evaluated by phenol hydrodeoxygenation as a probe reaction, and the optimal process conditions and reusability of the catalytic reaction were studied. The results showed that under 3MPa and 623K, Mo-Ni / SPC catalyst showed excellent catalytic performance, with a phenol conversion rate of 98%, a cyclohexane selectivity of about 95%, and a deoxygenation rate of 100%. This technology has some similarities with the patent technology I applied for. He removes oxygen from phenol, while this patent removes oxygen from oils and fats. This patent also has a hydrogenation function to produce diesel, and the application fields are different.

[0008] Chinese Patent Application No. 201711043323.9 Lou Hui et al. disclosed a catalyst for oil hydrodeoxygenation reaction and its preparation method. The carrier is different. The carrier he used is walnut shell, and the target product reaches up to 98.3%. The carrier used in this patent is montmorillonite, which is better than his, and the target product reaches 99.1%. There are very few literatures and materials on the preparation of hydrodeoxygenation catalysts using montmorillonite as raw material.

[0009] In view of the shortcomings of the above catalysts, a low-cost, high-activity and high-stability hydrodeoxygenation catalyst was prepared using acid-modified montmorillonite as a carrier, which has been improved in terms of stability, selectivity and activity. Summary of the invention

[0010] The core technology of oil hydrogenation to produce biodiesel is mainly hydrogenation catalysts, including hydrodeoxygenation and hydroisomerization catalysts. Hydroisomerization reaction refers to the reaction of isomerizing straight-chain alkanes to isoalkanes in the presence of hydrogen. On metal-acid bifunctional catalysts, the hydrogenation-deoxygenation reaction takes place on the metal active center, and the isomerization reaction takes place on the acid center.

[0011] The main components of animal and vegetable oils are triglycerides, in which the fatty acid chain length is generally C 12 ~C 24 , with C 16 and C 18 Most of them are fatty acids. Typical fatty acids are saturated acids (palmitic acid, stearic acid), monounsaturated acids (oleic acid) and polyunsaturated acids (linoleic acid, linolenic acid). The degree of unsaturation varies greatly with the type of oil. Under catalytic hydrogenation conditions, triglycerides first undergo hydrogenation saturation of unsaturated acids, and further crack to form intermediate products including diglyceric acid, monoglyceric acid and carboxylic acid, and then undergo hydrogenation decarboxylation, hydrogenation decarbonylation and hydrogenation deoxygenation to form normal alkanes. The main product of the reaction is C 12 ~C 24 Normal alkanes, by-products include propane, water and a small amount of CO and CO2. The reaction principle of the hydrodeoxygenation process of animal and vegetable oils is shown in the following formula:

[0012]

[0013] The balance between the hydrogenation-dehydrogenation activity of the metal components and the acidity of the zeolite is crucial, which determines the reaction process of n-alkane isomerization, thereby affecting the activity, stability, selectivity and distribution of the catalyst.

[0014] In view of the fact that there is no report on the use of montmorillonite as a raw material to prepare a catalyst carrier, the purpose of the present invention is to provide a montmorillonite carrier and a preparation method thereof, a preparation method of a hydrodeoxygenation catalyst and its application. The preparation method uses acid-modified montmorillonite as a raw material to prepare a montmorillonite carrier. The preparation method is low in cost, and the hydrodeoxygenation catalyst prepared from the montmorillonite carrier has the advantages of high activity and high stability. The hydrodeoxygenation catalyst is improved in terms of stability, selectivity and activity.

[0015] To achieve the above purpose, the present invention provides a method for preparing a montmorillonite carrier, which comprises: modifying the montmorillonite by acidification with an acidifier, then adding a crosslinking agent to carry out a crosslinking reaction, and calcining to obtain the montmorillonite carrier.

[0016] The method for preparing a montmorillonite carrier of the present invention comprises the following: the montmorillonite is at least one of sodium-based montmorillonite, calcium-based montmorillonite, magnesium-based montmorillonite and sodium-calcium-based montmorillonite.

[0017] In the method for preparing a montmorillonite carrier of the present invention, the acidulant is at least one of H2SO4, HCl, H3PO4, HNO3, and HClO4, preferably HCl or H3PO4; the mass concentration of the acidulant is 5 to 40 wt%, preferably 10 to 20 wt%.

[0018] In the method for preparing the montmorillonite carrier of the present invention, the solid-liquid ratio of the montmorillonite to the acidifier is 1:10-20.

[0019] In the method for preparing the montmorillonite carrier of the present invention, the temperature of the acidification modification is 40-95° C. and the time is 2-5 hours.

[0020] The preparation method of the montmorillonite carrier of the present invention, the cross-linking agent is an aluminum cross-linking agent, the cross-linking agent is an aluminum cross-linking agent, and the addition amount of the aluminum cross-linking agent is 2-6 mmolAl 3+ / g montmorillonite.

[0021] In the method for preparing the montmorillonite carrier of the present invention, the calcination temperature is 500-600° C. and the calcination time is 3-6 hours.

[0022] In the method for preparing the montmorillonite carrier of the present invention, the temperature of the cross-linking reaction is 60° C. to 95° C., and the time is 2 to 10 hours.

[0023] The preparation method of the montmorillonite carrier of the present invention further adds an auxiliary agent during the preparation process, wherein the auxiliary agent is at least one of methyl cellulose, citric acid and sesbania powder; the mass ratio of the auxiliary agent to the montmorillonite is 3-11.5:100.

[0024] Preferably, the preparation method of the montmorillonite carrier of the present invention can also be described in detail as follows:

[0025] (1) Preparation of cross-linking agent:

[0026] Under vigorous stirring, NH3·H2O solution (NH3 / AlCl3 solution) was added dropwise. 3+ The molar ratio is 2 to 2.4), and the pH value of the solution is always maintained between 3.5 and 6 during the dropwise addition process. The solution is then placed in a constant temperature water bath at 60°C to 95°C overnight and aged for more than 10 hours.

[0027] (2) Preparation of acidified montmorillonite suspension:

[0028] The montmorillonite is added into a sulfuric acid solution with a mass concentration of 5-40wt%, and stirred at 40-95°C for 2-5h to fully expand the montmorillonite to obtain a montmorillonite suspension.

[0029] (3) Preparation of cross-linked montmorillonite:

[0030] The pH value of the montmorillonite suspension in step (2) is adjusted to 3.5-6, and 2-6 mmol Al 3+ / g soil ratio, add the prepared aluminum crosslinking agent dropwise, maintain 60℃ to 95℃ for 2-10h, and let stand overnight. Discard the supernatant, remove the sand deposited at the bottom, filter, wash until there is no Cl-, dry the filter cake at 80-105℃ to constant weight, grind it into powder, and roast it at 400℃ for 4h to obtain crosslinked montmorillonite.

[0031] (4) Preparation of montmorillonite carrier:

[0032] Cross-linked montmorillonite, 0.5ω% to 5.0ω% methylcellulose, 1.0ω% to 3.0ω% citric acid, and 1.5ω% to 3.5ω% sesbania powder are uniformly mixed to obtain a mixed dry powder, small-pore alumina is weighed according to a mass ratio of small-pore alumina to dry powder of 1:5.7 to 9, nitric acid is weighed according to a mass ratio of nitric acid to mixed material of 1:0.2 to 2, and deionized water is weighed according to a mass ratio of deionized water to mixed material of 1:1.1 to 2, the weighed materials are mixed, stirred uniformly, and then mixed and kneaded with the dry powder, extruded into a cylindrical shape, dried at 80 to 120° C. for 6 to 8 hours, and roasted at 500 to 600° C. for 3 to 6 hours to obtain a formed montmorillonite carrier. The present invention also provides a montmorillonite carrier obtained by the above preparation method.

[0033] The present invention further provides a method for preparing a hydrodeoxygenation catalyst, which comprises: loading the montmorillonite carrier obtained by the above-mentioned method for preparing the montmorillonite carrier in an active metal solution, aging, drying and calcining to obtain the hydrodeoxygenation catalyst.

[0034] In the preparation method of the hydrodeoxygenation catalyst of the present invention, the active metal is at least one of Group VIIIB metals and Group VIB metals, preferably nickel and molybdenum.

[0035] The preparation method of the hydrodeoxygenation catalyst of the present invention comprises the following components based on 100% mass of the hydrodeoxygenation catalyst: 2.0wt%-10.0wt% of nickel oxide, 15.0wt%-20.0wt% of aluminum oxide, 5.0wt%-30.0wt% of molybdenum oxide, and 0.5wt%-5.0wt% of phosphorus pentoxide.

[0036] In the preparation method of the hydrodeoxygenation catalyst of the present invention, the aging time is 8 hours to 36 hours.

[0037] In the preparation method of the hydrodeoxygenation catalyst of the present invention, the drying temperature is 70° C. to 150° C., and the drying time is 5 h to 16 h.

[0038] In the preparation method of the hydrodeoxygenation catalyst of the present invention, the calcination temperature is 400° C. to 600° C., and the calcination time is 2 h to 10 h.

[0039] Preferably, the preparation method of the hydrodeoxygenation catalyst of the present invention can also be described in detail as follows:

[0040] One or more montmorillonite selected from sodium montmorillonite, calcium montmorillonite, magnesium montmorillonite and sodium-calcium montmorillonite is used as a raw material, and the montmorillonite acidified, activated, dried and cross-linked by H2SO4 with a mass concentration of 5-40% is used as a carrier, and nickel, molybdenum and phosphorus are loaded by an equal volume co-impregnation method, and the loading amount of nickel oxide is 2.0ω%-10.0ω%, aluminum oxide is 15.0ω%-20.0ω%, molybdenum oxide is 5.0ω%-30.0ω%, and phosphorus pentoxide is 0.5ω%-5.0ω%. The catalyst is co-impregnated and aged for 8h-36h under natural conditions, dried at 70℃-150℃ for 5h-16h, then roasted at 400℃-600℃ for 2h-10h, and naturally cooled to room temperature to obtain a catalyst.

[0041] The present invention further provides an application of the above hydrodeoxygenation catalyst in the preparation of biodiesel by hydrogenation of animal and vegetable fats. The hydrodeoxygenation catalyst prepared by the present invention is suitable for hydrogenating various qualities of animal and vegetable fats into high-quality biodiesel fractions, and can be used in the field of refined phenol.

[0042] The present invention has the following advantages and effects:

[0043] The present invention uses acid-modified montmorillonite as a raw material, and performs a cross-linking reaction to prepare a montmorillonite carrier. The preparation method has low cost, and the hydrodeoxygenation catalyst prepared from the montmorillonite carrier has the advantages of high activity, high stability, etc. The hydrodeoxygenation catalyst is improved in terms of stability, selectivity, and activity. The modified montmorillonite material of the present invention forms a multi-layer through-channel structure, while overcoming the disadvantage of poor hydrothermal stability caused by the large amount of aluminum oxide used in the preparation of conventional hydrodeoxygenation catalysts. The modified montmorillonite provides a channel space that is very beneficial to the hydrodeoxygenation of bio-lipid macromolecules. DETAILED DESCRIPTION

[0044] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.

[0045] Example 1

[0046] 1. Preparation of montmorillonite carrier precursor:

[0047] (1) Preparation of cross-linking agent:

[0048] Weigh AlCl3·6H2O (0.08 mol, 19.28 g) and add 400 mL of water to make a 0.2 mol / L aqueous solution. Weigh 26% ammonia water (0.192 mol, 12.55 mL) and add 960 mL of water to make a 0.2 mol / L ammonia solution. At 65°C, drop NH3·H2O solution (NH3 / AlCl3) into the vigorously stirred AlCl3 solution (0.2 mol / L). 3+ The molar ratio is 2 to 2.4), and the addition is completed after 2 hours. The pH value of the solution is always maintained between 3.5 and 6. Then it is placed in a constant temperature water bath at 60°C to 95°C overnight and aged for more than 10 hours.

[0049] (2) Preparation of acidified montmorillonite suspension:

[0050] Take 200g of API-4 sodium-calcium montmorillonite and add it into 40%wt, 2000mL HCl solution, and stir it at 50℃ for 4h to make the montmorillonite fully expand.

[0051] (3) Preparation of cross-linked montmorillonite:

[0052] The API-4 sodium-calcium montmorillonite suspension in step (2) was adjusted to a pH of 3.5 to 6 with concentrated hydrochloric acid, and then heated to 60 to 95°C with 2 mmol Al 3+ / g soil ratio, add the prepared aluminum crosslinking agent dropwise, maintain stirring at 60℃ for 2h after the addition is complete, and let it stand overnight. Discard the supernatant, remove the sand deposited at the bottom, filter, wash until there is no Cl-, dry the filter cake at 105℃ to constant weight, grind it into powder, and roast it at 400℃ for 4h.

[0053] 2. Preparation of montmorillonite carrier:

[0054] Weigh 57g of acidified montmorillonite powder, 2.1g of methyl cellulose, 1.4g of citric acid, and 2.0g of sesbania powder, mix the dry powders evenly, take 3.4g of nitric acid and add it dropwise to 70g of deionized water, add 17.187g of small-pore alumina to the deionized water, stir evenly, then mix with the dry powder, extrude into a cylinder, dry at 80°C for 8h, and calcine at 500°C for 3h to obtain a shaped carrier.

[0055] 3. Preparation of hydrodeoxygenation catalyst:

[0056] The catalyst was prepared by equal volume co-impregnation method: 8.1 g nickel nitrate, 11.0 g ammonium molybdate and 2.8 g phosphoric acid were prepared into an aqueous solution. The shaped carrier was impregnated and aged for 10 h in the co-impregnation solution, dried at 95 °C for 10 h, and calcined at 450 °C for 3.5 h to obtain the catalyst.

[0057] 4. Catalyst evaluation:

[0058] Weigh 10.0 mL of catalyst, load it into a continuous flow fixed bed reactor, and sulfide it at 320 ° C for 6 h. Control the reaction temperature to 375 ° C, the reaction pressure to 4.0 MPa, the reaction hydrogen to oil ratio to 1000:1, and the reaction space velocity to 0.8 h -1 In a hydrogen atmosphere, with n-octane as solvent, the deoxygenation rate of tung oil with an oxygen content of 12.6ω% is about 99.92ω under the action of montmorillonite hydrogenation deoxygenation catalyst, and the liquid products are biodiesel and water. After separating the water, sampling and analysis show that the contents of pentadecane, hexadecane, heptadecane and octadecane are up to 98ω, and the appearance is colorless and transparent.

[0059] Example 2

[0060] 1. Preparation of montmorillonite carrier precursor:

[0061] (1) Preparation of cross-linking agent:

[0062] Weigh AlCl3·6H2O (0.08 mol, 19.28 g) and add 400 mL of water to make a 0.2 mol / L aqueous solution. Weigh 26% ammonia water (0.192 mol, 12.55 mL) and add 960 mL of water to make a 0.2 mol / L ammonia solution. At 65°C, drop NH3·H2O solution (NH3 / AlCl3) into the vigorously stirred AlCl3 solution (0.2 mol / L). 3+ The molar ratio is 2 to 2.4), and the addition is completed after 2 hours. The pH value of the solution is always maintained between 3.5 and 6. Then it is placed in a constant temperature water bath at 60°C to 95°C overnight and aged for more than 10 hours.

[0063] (2) Preparation of acidified montmorillonite suspension:

[0064] Take 150g of API-4 sodium montmorillonite and add it into 5%wt, 2000mL sulfuric acid solution, and stir it at 50℃ for 4h to make the montmorillonite fully expand.

[0065] (3) Preparation of cross-linked montmorillonite:

[0066] The API-4 sodium montmorillonite suspension in step (2) was adjusted to a pH of 3.5-6 with concentrated hydrochloric acid and heated to 60°C to 95°C with 6 mmol Al 3+ / g soil ratio, add the prepared aluminum crosslinking agent dropwise, maintain stirring at 60℃ for 2h after the addition is complete, and let it stand overnight. Discard the supernatant, remove the sand deposited at the bottom, filter, wash until there is no Cl-, dry the filter cake at 105℃ to constant weight, grind it into powder, and roast it at 400℃ for 4h.

[0067] 2. Preparation of montmorillonite carrier:

[0068] Weigh 40.0g of montmorillonite, 0.8g of methyl cellulose, 0.9g of citric acid, and 1.2g of sesbania powder, mix the dry powders evenly, take 1.6g of nitric acid and add it dropwise to 40.0g of deionized water, add 11.28g of small pore alumina to the deionized water, stir evenly, then mix with the dry powders, extrude into a cylinder, dry at 80°C for 7h, and calcine at 550°C for 3h to obtain a shaped carrier.

[0069] 3. Preparation of hydrodeoxygenation catalyst:

[0070] The catalyst was prepared by equal volume co-impregnation method: 7.6 g nickel nitrate, 12 g ammonium molybdate and 0.5 g phosphoric acid were prepared into an aqueous solution. The shaped carrier was impregnated and aged for 12 h in the co-impregnation solution, dried at 100 °C for 7 h, and calcined at 500 °C for 3 h to obtain the catalyst.

[0071] 4. Catalyst evaluation:

[0072] Weigh 10.0 mL of catalyst, load it into a continuous flow fixed bed reactor, and sulfide it at 320 ° C for 6 h. Control the reaction temperature to 360 ° C, the reaction pressure to 5.0 MPa, the reaction hydrogen-oil ratio to 800:1, and the reaction space velocity to 1.2 h -1 In a hydrogen atmosphere, with dodecane as solvent and non-edible grade palm oil with an oxygen content of 12.2ω% under the action of montmorillonite hydrodeoxygenation catalyst, the deoxygenation rate is about 99.91ω%, and the liquid products are biodiesel and water. After separating the water, sampling and analysis show that the contents of pentadecane, hexadecane, heptadecane and octadecane reach 95.6ω, and the appearance is colorless and transparent.

[0073] Example 3

[0074] 1. Preparation of montmorillonite carrier precursor:

[0075] (1) Preparation of cross-linking agent:

[0076] Weigh AlCl3·6H2O (0.08 mol, 19.28 g) and add 400 mL of water to make a 0.2 mol / L aqueous solution. Weigh 26% ammonia water (0.192 mol, 12.55 mL) and add 960 mL of water to make a 0.2 mol / L ammonia solution. At 65°C, drop NH3·H2O solution (NH3 / AlCl3) into the vigorously stirred AlCl3 solution (0.2 mol / L). 3+ The molar ratio is 2 to 2.4), and the addition is completed after 2 hours. The pH value of the solution is always maintained between 3.5 and 6. Then it is placed in a constant temperature water bath at 60°C to 95°C overnight and aged for more than 10 hours.

[0077] (2) Preparation of acidified montmorillonite suspension:

[0078] Take 200g of API-4 calcium-based montmorillonite and add it into 15%wt, 2000mL sulfuric acid solution, and stir it at 80℃ for 4h to make the montmorillonite fully expand.

[0079] (3) Preparation of cross-linked montmorillonite:

[0080] The API-4 calcium-based montmorillonite suspension in step (2) was adjusted to pH 5 with concentrated hydrochloric acid and heated at 80°C with 4 mmol Al 3+ / g soil ratio, add the prepared aluminum crosslinking agent dropwise, maintain stirring at 80℃ for 2h after the addition is complete, and let it stand overnight. Discard the supernatant, remove the sand deposited at the bottom, filter, wash until there is no Cl-, dry the filter cake at 105℃ to constant weight, grind it into powder, and roast it at 400℃ for 4h.

[0081] 2. Preparation of montmorillonite carrier:

[0082] Weigh 19.4 g of montmorillonite powder, 0.6 g of methyl cellulose, 0.7 g of citric acid, and 0.8 g of sesbania powder, mix the dry powders evenly, take 0.7 g of nitric acid and add it dropwise to 25.0 g of deionized water, add 8 g of small-pore alumina to the deionized water, stir evenly, and then mix with the dry powders, extrude into a cylindrical shape, dry at 90°C for 8 h, and calcine at 600°C for 4 h to obtain a shaped carrier.

[0083] 3. Preparation of hydrodeoxygenation catalyst:

[0084] The catalyst was prepared by equal volume co-impregnation method: 8.2 g nickel nitrate, 7.6 g ammonium molybdate and 0.45 g phosphoric acid were prepared into an aqueous solution. The shaped carrier was impregnated and aged for 15 h in the co-impregnation solution, dried at 110 °C for 6 h, and calcined at 550 °C for 3 h to obtain the catalyst.

[0085] 4. Catalyst evaluation:

[0086] Weigh 10.0 mL of catalyst, load it into a continuous flow fixed bed reactor, and sulfide it at 320 ° C for 6 h. Control the reaction temperature to 355 ° C, the reaction pressure to 6.0 MPa, the reaction hydrogen-oil ratio to 1000:1, and the reaction space velocity to 1.5 h -1 In a hydrogen atmosphere, with n-heptane as solvent, the deoxygenation rate of waste cooking oil with an oxygen content of 12.9ω% is about 99.91ω under the action of montmorillonite hydrodeoxygenation catalyst. The liquid products are biodiesel and water. After separating the water, sampling and analysis show that the contents of pentadecane, hexadecane, heptadecane and octadecane reach 95ω, and the appearance is colorless and transparent.

[0087] Example 4

[0088] 1. Preparation of montmorillonite carrier precursor:

[0089] (1) Preparation of cross-linking agent:

[0090] Weigh AlCl3·6H2O (0.08 mol, 19.28 g) and add 400 mL of water to make a 0.2 mol / L aqueous solution. Weigh 26% ammonia water (0.192 mol, 12.55 mL) and add 960 mL of water to make a 0.2 mol / L ammonia solution. At 65°C, drop NH3·H2O solution (NH3 / AlCl3) into the vigorously stirred AlCl3 solution (0.2 mol / L). 3+ The molar ratio is 2 to 2.4), and the addition is completed after 2 hours. The pH value of the solution is always maintained between 3.5 and 6. Then it is placed in a constant temperature water bath at 60°C to 95°C overnight and aged for more than 10 hours.

[0091] (2) Preparation of acidified montmorillonite suspension:

[0092] Take 150g of API-4 sodium-calcium montmorillonite and add it into 15%wt, 2000mL sulfuric acid solution, and stir it at 70℃ for 4h to make the montmorillonite fully expand.

[0093] (3) Preparation of cross-linked montmorillonite;

[0094] The API-4 sodium-calcium montmorillonite suspension in step (2) was adjusted to pH 6 with concentrated hydrochloric acid and heated to 4 mmol Al 3+ / g soil ratio, add the prepared aluminum crosslinking agent dropwise, maintain stirring at 60℃ for 2h after the addition is complete, and let it stand overnight. Discard the supernatant, remove the sand deposited at the bottom, filter, wash until there is no Cl-, dry the filter cake at 105℃ to constant weight, grind it into powder, and roast it at 400℃ for 4h.

[0095] 2. Preparation of montmorillonite carrier:

[0096] Weigh 60g of montmorillonite, 1.3g of methyl cellulose, 1.5g of citric acid, and 1.9g of sesbania powder, mix the dry powders evenly, take 2g of nitric acid and add it dropwise to 72.0g of deionized water, add 17.10g of small pore alumina to the deionized water, stir evenly, then mix with the dry powders, extrude into a cylindrical shape, dry at 120°C for 6h, and calcine at 500°C for 6h to obtain a shaped carrier.

[0097] 3. Preparation of hydrodeoxygenation catalyst:

[0098] The catalyst was prepared by equal volume co-impregnation method: 30.3 g nickel nitrate, 16.3 g ammonium molybdate and 2.2 g phosphoric acid were prepared into an aqueous solution, the shaped carrier was impregnated and aged for 24 h in the co-impregnation solution, dried at 150°C for 5 h, and calcined at 600°C for 2 h to obtain the catalyst.

[0099] 4. Catalyst evaluation:

[0100] Weigh 10.0 mL of catalyst, load it into a continuous flow fixed bed reactor, and sulfide it at 320 ° C for 6 h. Control the reaction temperature to 375 ° C, the reaction pressure to 4.5 MPa, the reaction hydrogen to oil ratio to 800:1, and the reaction space velocity to 0.5 h -1 In a hydrogen atmosphere, with undecane as solvent, tung oil with an oxygen content of 12.6ω% is deoxygenated at a rate of about 99.93ω under the action of montmorillonite catalyst for hydrogenation and deoxygenation. The liquid products are biodiesel and water. After separating the water, the samples are analyzed and the contents of pentadecane, hexadecane, heptadecane and octadecane are as high as 99.1ω. The appearance is colorless and transparent.

[0101] Comparative Example 1

[0102] 1. Preparation of montmorillonite carrier precursor:

[0103] (1) Preparation of acidified montmorillonite suspension:

[0104] Take 200g of API-4 calcium-based montmorillonite and add it into 15%wt, 2000mL sulfuric acid solution, and stir it at 80℃ for 4h to make the montmorillonite fully expand.

[0105] (2) Discard the supernatant, remove the sand and soil deposited at the bottom, filter, wash, dry the filter cake at 105°C to constant weight, grind it into powder, and calcine it at 400°C for 4h.

[0106] 2. Preparation of montmorillonite carrier:

[0107] Weigh 9.4 g of montmorillonite powder, 0.6 g of methyl cellulose, 0.7 g of citric acid, and 0.8 g of sesbania powder, mix the dry powders evenly, take 0.7 g of nitric acid and add it dropwise to 25.0 g of deionized water, add 8 g of small pore alumina to the deionized water, stir evenly, then mix with the dry powders, extrude into a cylindrical shape, dry at 90°C for 8 h, and calcine at 600°C for 4 h to obtain a shaped carrier.

[0108] 3. Metal loading of catalyst:

[0109] The catalyst was prepared by equal volume co-impregnation method: 8.2 g nickel nitrate, 7.6 g ammonium molybdate and 0.45 g phosphoric acid were prepared into an aqueous solution. The shaped carrier was impregnated and aged for 15 h in the co-impregnation solution, dried at 110 °C for 6 h, and calcined at 550 °C for 3 h to obtain the catalyst.

[0110] 4. Catalyst evaluation:

[0111] Weigh 10.0 mL of catalyst, load it into a continuous flow fixed bed reactor, and sulfide it at 320 ° C for 6 h. Control the reaction temperature to 355 ° C, the reaction pressure to 6.0 MPa, the reaction hydrogen-oil ratio to 1000:1, and the reaction space velocity to 1.5 h -1 In a hydrogen atmosphere, with n-heptane as solvent, the oxygen content of waste cooking oil is 12.9ω%, and the oxygen removal rate is only 67ω under the action of montmorillonite hydrodeoxygenation catalyst. The liquid products are biodiesel and water. After separating the water, sampling and analysis show that the content of pentadecane, hexadecane, heptadecane and octadecane is 58.1ω, and the appearance is colorless and transparent.

[0112] Comparative Example 2

[0113] 1. Preparation of montmorillonite carrier precursor:

[0114] (1) Preparation of montmorillonite suspension:

[0115] Take 150g of API-4 sodium montmorillonite and add it into 2000mL of deionized water. Stir it at 50℃ for 4h to make the montmorillonite fully expand.

[0116] (2) Discard the supernatant, remove the sand and soil deposited at the bottom, filter, wash, dry the filter cake at 105°C to constant weight, grind it into powder, and calcine it at 400°C for 4h.

[0117] 2. Preparation of montmorillonite carrier:

[0118] Weigh 40.0g of montmorillonite, 0.8g of methyl cellulose, 0.9g of citric acid, and 1.2g of sesbania powder, mix the dry powders evenly, take 1.6g of nitric acid and add it dropwise to 40.0g of deionized water, add 11.28g of small pore alumina to the deionized water, stir evenly, then mix with the dry powders, extrude into a cylinder, dry at 80°C for 7h, and calcine at 550°C for 3h to obtain a shaped carrier.

[0119] 3. Metal loading of catalyst:

[0120] The catalyst was prepared by equal volume co-impregnation method: 7.6 g nickel nitrate, 12 g ammonium molybdate and 0.5 g phosphoric acid were prepared into an aqueous solution. The shaped carrier was impregnated and aged for 12 h in the co-impregnation solution, dried at 100 °C for 7 h, and calcined at 500 °C for 3 h to obtain the catalyst.

[0121] 4. Catalyst evaluation:

[0122] Weigh 10.0 mL of catalyst, load it into a continuous flow fixed bed reactor, and sulfide it at 320 ° C for 6 h. Control the reaction temperature to 360 ° C, the reaction pressure to 5.0 MPa, the reaction hydrogen-oil ratio to 800:1, and the reaction space velocity to 1.2 h -1 In a hydrogen atmosphere, with dodecane as solvent, the oxygen content of non-edible palm oil with a 12.2ω% oxygen content was removed by montmorillonite catalyst, and the oxygen removal rate was only 58ω. The liquid products were biodiesel and water. After separating the water, the samples were analyzed and the contents of pentadecane, hexadecane, heptadecane and octadecane reached 48.1ω. The appearance was colorless and transparent.

[0123] Example 5

[0124] 1. Preparation of montmorillonite carrier precursor:

[0125] (1) Preparation of cross-linking agent:

[0126] Weigh AlCl3·6H2O (0.08 mol, 19.28 g) and add 400 mL of water to make a 0.2 mol / L aqueous solution. Weigh 26% ammonia water (0.192 mol, 12.55 mL) and add 960 mL of water to make a 0.2 mol / L ammonia solution. At 65°C, drop NH3·H2O solution (NH3 / AlCl3) into the vigorously stirred AlCl3 solution (0.2 mol / L). 3+ The molar ratio is 2 to 2.4), and the addition is completed after 2 hours. The pH value of the solution is always maintained between 3.5 and 6. Then it is placed in a constant temperature water bath at 60°C to 95°C overnight and aged for more than 10 hours.

[0127] (2) Preparation of acidified montmorillonite suspension:

[0128] Take 100g of API-4 calcium-based montmorillonite and add it into 15%wt, 2000mL H3PO4 solution, and stir it at 50℃ for 4h to make the montmorillonite fully expand.

[0129] (3) Preparation of cross-linked montmorillonite:

[0130] The API-4 calcium-based montmorillonite suspension in step (2) was adjusted to a pH of 3.5-6 with concentrated hydrochloric acid and heated to 60°C to 95°C with 4 mmol Al 3+ / g soil ratio, add the prepared aluminum crosslinking agent dropwise, maintain stirring at 60℃ for 2h after the addition is complete, and let it stand overnight. Discard the supernatant, remove the sand deposited at the bottom, filter, wash until there is no Cl-, dry the filter cake at 105℃ to constant weight, grind it into powder, and roast it at 400℃ for 4h.

[0131] 2. Preparation of montmorillonite carrier:

[0132] Weigh 40.0g of montmorillonite, 0.8g of methyl cellulose, 0.9g of citric acid, and 1.2g of sesbania powder, mix the dry powders evenly, take 1.6g of nitric acid and add it dropwise to 40.0g of deionized water, add 11.28g of small pore alumina to the deionized water, stir evenly, then mix with the dry powders, extrude into a cylinder, dry at 80°C for 7h, and calcine at 550°C for 3h to obtain a shaped carrier.

[0133] 3. Preparation of hydrodeoxygenation catalyst:

[0134] The catalyst was prepared by equal volume co-impregnation method: 7.6 g nickel nitrate, 12 g ammonium molybdate and 0.5 g phosphoric acid were prepared into an aqueous solution. The shaped carrier was impregnated and aged for 12 h in the co-impregnation solution, dried at 100 °C for 7 h, and calcined at 500 °C for 3 h to obtain the catalyst.

[0135] 4. Catalyst evaluation:

[0136] Weigh 10.0 mL of catalyst, load it into a continuous flow fixed bed reactor, and sulfide it at 320 ° C for 6 h. Control the reaction temperature at 345 ° C, the reaction pressure at 3.0 MPa, the reaction hydrogen-oil ratio at 800:1, and the reaction space velocity at 1.2 h -1 In a hydrogen atmosphere, 2-methylbenzofuran with an oxygen content of 12.12ω% is deoxygenated over montmorillonite catalyst with a deoxygenation rate of about 99.91ω, and the main products are propylbenzene and propylcyclohexane.

[0137] Example 6

[0138] Evaluation of the Deoxygenation Catalyst Prepared in Example 5 for Deoxygenation of Acetophenone

[0139] Weigh 10.0 mL of catalyst, load it into a continuous flow fixed bed reactor, and sulfide it at 320 ° C for 6 h. Control the reaction temperature at 345 ° C, the reaction pressure at 3.0 MPa, the reaction hydrogen-oil ratio at 800:1, and the reaction space velocity at 1.2 h -1 In a hydrogen atmosphere, acetophenone with an oxygen content of 13.32ω% is deoxygenated at a rate of about 99.92ω over the action of montmorillonite hydrodeoxygenation catalyst, and the main products are ethylbenzene and ethylcyclohexane.

[0140] Comparative Example 3

[0141] 1. Preparation of montmorillonite carrier precursor:

[0142] (1) Preparation of cross-linking agent:

[0143] Weigh AlCl3·6H2O (0.08 mol, 19.28 g) and add 400 mL of water to make a 0.2 mol / L aqueous solution. Weigh 26% ammonia water (0.192 mol, 12.55 mL) and add 960 mL of water to make a 0.2 mol / L ammonia solution. At 65°C, drop NH3·H2O solution (NH3 / AlCl3) into the vigorously stirred AlCl3 solution (0.2 mol / L). 3+ The molar ratio is 2 to 2.4), and the addition is completed after 2 hours. The pH value of the solution is always maintained between 3.5 and 6. Then it is placed in a constant temperature water bath at 60°C to 95°C overnight and aged for more than 10 hours.

[0144] (2) Preparation of montmorillonite suspension:

[0145] Take 150g of API-4 sodium-calcium montmorillonite and add it into 2000mL of deionized water. Stir it at 70℃ for 4h to make the montmorillonite fully expand.

[0146] (3) Preparation of cross-linked montmorillonite;

[0147] The API-4 sodium-calcium montmorillonite suspension of step (2) was heated to 60°C to 95°C with 4 mmol Al 3+ / g soil ratio, add the prepared aluminum crosslinking agent dropwise, maintain stirring at 60℃ for 2h after the addition is complete, and let it stand overnight. Discard the supernatant, remove the sand deposited at the bottom, filter, wash until there is no Cl-, dry the filter cake at 105℃ to constant weight, grind it into powder, and roast it at 400℃ for 4h.

[0148] 2. Preparation of montmorillonite carrier:

[0149] Weigh 60g of montmorillonite, 1.3g of methyl cellulose, 1.5g of citric acid, and 1.9g of sesbania powder, mix the dry powders evenly, take 2g of nitric acid and add it dropwise to 72.0g of deionized water, add 17.10g of small pore alumina to the deionized water, stir evenly, then mix with the dry powders, extrude into a cylindrical shape, dry at 120°C for 6h, and calcine at 500°C for 6h to obtain a shaped carrier.

[0150] 3. Preparation of hydrodeoxygenation catalyst:

[0151] The catalyst was prepared by equal volume co-impregnation method: 30.3 g nickel nitrate, 16.3 g ammonium molybdate and 2.2 g phosphoric acid were prepared into an aqueous solution, the shaped carrier was impregnated and aged for 24 h in the co-impregnation solution, dried at 150°C for 5 h, and calcined at 600°C for 2 h to obtain the catalyst.

[0152] 4. Catalyst evaluation:

[0153] Weigh 10.0 mL of catalyst, load it into a continuous flow fixed bed reactor, and sulfide it at 320 ° C for 6 h. Control the reaction temperature to 375 ° C, the reaction pressure to 4.5 MPa, the reaction hydrogen to oil ratio to 800:1, and the reaction space velocity to 0.5 h -1 In a hydrogen atmosphere, with undecane as solvent, the oxygen removal rate of tung oil with an oxygen content of 12.6ω% was only 75ω under the action of montmorillonite hydrodeoxygenation catalyst, and the liquid products were biodiesel and water. After separating the water, the samples were analyzed and the contents of pentadecane, hexadecane, heptadecane and octadecane reached 72.1ω. The appearance was colorless and transparent.

[0154] From the results of the above embodiments and comparative examples, it can be seen that after the montmorillonite of the present invention is acid-modified, the yields of pentadecane, hexadecane, heptadecane and octadecane are all higher than those of the comparative examples; in particular, from the comparison results of Example 3 and Comparative Example 1, Example 2 and Comparative Example 2, and Example 4 and Comparative Example 3, it can be seen that after the montmorillonite of the present invention is acid-modified or a cross-linking agent is added during the preparation process, the yields of pentadecane, hexadecane, heptadecane and octadecane can be significantly improved, but the montmorillonite of Comparative Example 2 is not acid-modified and a cross-linking agent is not added during the preparation process, and the yields of pentadecane, hexadecane, heptadecane and octadecane obtained are the worst; the montmorillonite of Comparative Example 1 is not acid-modified, and the montmorillonite of Comparative Example 3 is not acid-modified, and the yields of pentadecane, hexadecane, heptadecane and octadecane obtained are significantly lower than those of the embodiments of the present invention, and the deoxygenation rate of the embodiments of the present invention is much higher than that of the comparative examples. It can be proved that the montmorillonite of the present invention that is acid-modified or a cross-linking agent is added during the preparation process can significantly improve the activity and stability of the hydrodeoxygenation catalyst, and has a higher deoxygenation rate.

[0155] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.

Claims

1. Application of a hydrodeoxygenation catalyst in the hydrogenation of animal and vegetable oils to produce biodiesel, characterized in that: The preparation method of the hydrodeoxygenation catalyst comprises: impregnating a montmorillonite carrier in an active metal solution, aging, drying, and calcining to obtain a hydrodeoxygenation catalyst; the active metal is at least one of a Group VIII metal and a Group VIB metal; The preparation method of the montmorillonite carrier comprises: acidifying and modifying the montmorillonite by an acidifier, then adding a crosslinking agent to carry out a crosslinking reaction, and calcining to obtain the montmorillonite carrier; the crosslinking agent is an aluminum crosslinking agent.

2. The use according to claim 1, characterized in that: The montmorillonite is at least one of sodium-based montmorillonite, calcium-based montmorillonite, magnesium-based montmorillonite and sodium-calcium-based montmorillonite.

3. The use according to claim 1, characterized in that: The acidulant is at least one of H2SO4, HCl, H3PO4, HNO3, and HClO4; and the mass concentration of the acidulant is 5 to 40 wt%.

4. The use according to claim 3, characterized in that: The acidifier is HCl or H3PO4.

5. The use according to claim 3, characterized in that: The mass concentration of the acidulant is 10-20wt%.

6. The use according to claim 1, characterized in that: The solid-liquid ratio of the montmorillonite to the acidifier is 1:10-20; the addition amount of the aluminum crosslinking agent is 2-6 mmolAl 3+ / g montmorillonite.

7. The use according to claim 1, characterized in that: The temperature of the acid modification is 40-95°C, and the time is 2-5 hours; the temperature of the calcination is 500-600°C, and the time is 3-6 hours; the temperature of the cross-linking reaction is 60-95°C, and the time is 2-10 hours.

8. The use according to claim 1, characterized in that: An auxiliary agent is also added in the preparation method of the montmorillonite carrier, and the auxiliary agent is at least one of methyl cellulose, citric acid and sesbania powder; the mass ratio of the auxiliary agent to the montmorillonite is 3-11.5:

100.

9. The use according to claim 1, characterized in that: The active metals are nickel and molybdenum.

10. The use according to claim 1, characterized in that: Based on 100% by mass of the hydrodeoxygenation catalyst, the hydrodeoxygenation catalyst includes the following components: 2.0 wt % to 10.0 wt % of nickel oxide, 15.0 wt % to 20.0 wt % of aluminum oxide, 5.0 wt % to 30.0 wt % of molybdenum oxide, and 0.5 wt % to 5.0 wt % of phosphorus pentoxide.