A preparation method of MgAl hydrotalcite catalyst and its application in the preparation of 1,1,1,3,3-pentachloropropane

By cationically doped modified MgAl hydrotalcite catalyst and combined with sodium dodecyl sulfate modification, the problems of low catalytic activity and complex process in the prior art were solved, and high-efficiency and low-cost 1,1,1,3 ,3-pentachloropropane synthesis, the catalyst can be reused, safe and environmentally friendly.

CN116408091BActive Publication Date: 2024-11-19ZHEJIANG WEITONG CATALYTIC NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210455852.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-27
Publication Date
2024-11-19
Estimated Expiration
2042-04-27

AI Technical Summary

Technical Problem

The prior art in the synthesis of 1,1,1,3,3-pentachloropropane using carbon tetrachloride and vinyl chloride as raw materials is low in catalytic activity, the catalytic process is complex, and the addition of cocatalysts is required, which is complicated in operation, resulting in reaction efficiency. and less selectivity.

Method used

The MgAl hydrotalcite catalyst was prepared by co-precipitation method and cationically doped with copper salt. It was modified with sodium dodecyl sulfate as a support for catalysis, avoiding the addition of cocatalysts and organic solvents, and improving catalysis. Activity and selectivity.

Benefits of technology

It achieves high conversion and selectivity, and the catalyst can be recycled and used multiple times, with low cost, low pollution, safe and environmentally friendly, significantly improved catalytic effect, and a wider range of reaction temperature and acid-base.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003618697130000111
    Figure BDA0003618697130000111
  • Figure BDA0003618697130000121
    Figure BDA0003618697130000121
Patent Text Reader

Abstract

The present invention relates to the field of catalyst preparation, discloses a preparation method of MgAl hydrotalcite catalyst and its application in the preparation of 1,1,1,3,3-pentachloropropane, including the following steps: dissolving magnesium salt and aluminum salt in water to obtain mixed solution A; dissolving sodium hydroxide and sodium carbonate in water to obtain mixed solution B; reacting mixed solution A and mixed solution B by coprecipitation method to obtain mixed solution C; mixed solution C is filtered, washed and dried successively to obtain MgAl hydrotalcite catalyst; heating after mixing copper salt with MgAl hydrotalcite catalyst, then immersing in sodium dodecyl sulfate solution, then washing and drying to obtain cation-doped modified MgAl hydrotalcite catalyst, i.e. SDS / Cu / MgAl catalyst. The reaction conversion rate and selectivity of the catalyst in the present invention reach a high level, and can be recycled and used many times, has high reuse rate, low pollution, and is safe and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of catalyst preparation, and in particular to a method for preparing a MgAl hydrotalcite catalyst and application of the catalyst in preparing 1,1,1,3,3-pentachloropropane. Background Art

[0002] 1,1,1,3,3-pentafluoropropane is a very important chemical raw material with a wide range of applications. It is often used in the preparation of ozone-depleting foaming agents, refrigerants, cleaning agents, heat transfer media and aerosol propellers. It also serves as the best substitute in the polyurethane plastic foam industry. As an intermediate for the preparation of 1,1,1,3,3-pentafluoropropane (HFC-245fa), the preparation of 1,1,1,3,3-pentachloropropane (HCC-240fa) is particularly important. It has three mature synthesis routes, namely: (1) synthesis using carbon tetrachloride and 1,1-dichloroethylene as raw materials; (2) synthesis using carbon tetrachloride and ethylene as raw materials; (3) synthesis using carbon tetrachloride and vinyl chloride as raw materials. The first two synthesis methods are not one-step reactions, but multi-step reactions. Other by-products will be synthesized during the reaction process, reducing the overall yield of the reaction. In addition, in addition to increasing the waste of financial, human and material resources, it will also prolong the reaction time and increase the risk factor during the reaction process.

[0003] The invention patent with the publication number of WO1997037956A1 discloses a method for preparing a halogenated propane containing terminal fluorocarbon compounds, and provides a method for synthesizing 1,1,1,3,3-pentachloropropane from 1,1-dichloroethylene and carbon tetrachloride as raw materials. The reaction cannot be completed in one step, and other by-products will be produced in the process. In addition, in the synthesis process, since 1,1-dichloroethylene is not easy to store and transport, it is easy to polymerize in the reaction, resulting in a decrease in yield and process conversion rate. The reaction of 1,1-dichloroethylene will also cause damage to the experimental equipment.

[0004] The Chinese invention patent with publication number CN101260022A discloses a method for preparing 1,1,1,3,3-pentachloropropane, wherein the main catalyst is a copper organic complex R(OC6H3COO)Cu, wherein R is H, CH3, NH2 or COOH, the co-catalyst is an organic amine, and the solvent is acetonitrile or tert-butyl alcohol, and carbon tetrachloride and vinyl chloride are telomerized to produce 1,1,1,3,3-pentachloropropane. However, the conversion rate of vinyl chloride obtained by the method is 45%, the selectivity of 1,1,1,3,3-pentachloropropane is 49.89%, and the catalytic activity of the catalyst is low.

[0005] The Chinese invention patent application with publication number CN1213005C discloses a method for preparing 1,1,1,3,3-pentachloropropane, wherein cuprous chloride and various alcohol amines form a composite catalyst, and during the reaction, a small amount of a metal element selected from iron, cobalt, and nickel is added as a co-catalyst. This method requires the additional addition of a co-catalyst to achieve a better catalytic effect, and the reaction process needs to consider the proportion of the catalyst and the synergistic effect of the co-catalyst, and the operation process is relatively complicated. Summary of the invention

[0006] In order to solve the problems of low catalytic activity and complicated catalytic process in the process of synthesizing 1,1,1,3,3-pentachloropropane using carbon tetrachloride and vinyl chloride as raw materials, the present invention provides a preparation method of MgAl hydrotalcite catalyst and application of the catalyst in the preparation of 1,1,1,3,3-pentachloropropane. Hydrotalcite is used as a catalyst and is modified by cation doping without adding a co-catalyst, so that high conversion rate and reaction selectivity can be obtained, and the process steps are simple and the cost is low.

[0007] The specific technical scheme of the present invention is:

[0008] In a first aspect, the present invention provides a method for preparing a cation-doped modified MgAl hydrotalcite catalyst, comprising the following steps:

[0009] (1) dissolving a magnesium salt and an aluminum salt in water to obtain a mixed solution A; dissolving sodium hydroxide and sodium carbonate in water to obtain a mixed solution B; reacting the mixed solution A and the mixed solution B by a coprecipitation method to obtain a mixed solution C;

[0010] (2) The mixed solution C is filtered, washed, and dried in sequence to obtain a MgAl hydrotalcite catalyst;

[0011] (3) The copper salt and the MgAl hydrotalcite catalyst are mixed and heated, and then immersed in a modifier, and then washed and dried to obtain a cation-doped modified MgAl hydrotalcite catalyst.

[0012] Compared with other catalysts, the hydrotalcite catalyst of the present invention has the advantages of being able to be recycled and reused multiple times, having a high reuse rate, low pollution, safety and environmental protection, good catalytic effect, high conversion efficiency, and no need to add catalysts and other organic solvents. The reaction temperature range and reaction acidity and alkalinity are also wider. MgAl hydrotalcite is used as a carrier, copper salt is selected for cation doping, Cu 2+ Can replace part of Mg 2+, neither changing the layered structure distribution of magnesium-aluminum hydrotalcite nor reducing the influence of the Jiang-Taylor effect of copper-containing hydrotalcite. Copper compounds have a good catalytic effect on the preparation of 1,1,1,3,3-pentachloropropane by telomerization reaction. The copper salt-doped hydrotalcite catalyst does not require the addition of a co-catalyst, can achieve catalyst recycling, and reduce catalyst loss. In addition, under the synergistic catalytic influence of the three metal active components of copper, magnesium, and aluminum, the catalytic effect of the telomerization reaction of carbon tetrachloride and vinyl chloride to prepare 1,1,1,3,3-pentachloropropane is more excellent, and the reaction selectivity is also higher. In addition, the catalyst is also modified with sodium dodecyl sulfate to increase the solubility, and the conversion rate and selectivity of the telomerization reaction of carbon tetrachloride and polyethylene reach a high level.

[0013] Preferably, in step (1), the magnesium salt or aluminum salt is nitrate, chlorate, sulfate or acetate.

[0014] Preferably, in step (1), the molar ratio of the metal elements magnesium and aluminum in the mixed solution A may be 1:1, 2:1 or 3:1, more preferably 3:1; the molar ratios of sodium hydroxide and sodium carbonate in the mixed solution B follow the following formula: n(NaOH)=1.8*(Mg 2+ +Al 3+ ), n(Na2CO3)=2*(Mg 2+ ), where X 2+ Represents Mg 2+ The number of moles, where X 3+ Al 3+ The number of moles.

[0015] The hydrotalcite carriers formed by different magnesium-aluminum ratios have different catalytic effects. When the magnesium-aluminum ratio is 3:1, the formed hydrotalcite has a better effect, the interlayer spacing of the hydrotalcite becomes larger, the crystal form is well developed, the dispersion is good, the grain size is uniform, and the catalytic effect on cation doping is better.

[0016] Preferably, in step (1), the coprecipitation method is as follows: the base solution is prepared as an aqueous solution, mixed solution A and mixed solution B are added dropwise, and the pH is maintained at 9-10.

[0017] Preferably, in step (2), the drying is vacuum drying, the drying temperature is 60 to 90° C., and the drying time is 6 to 10 hours.

[0018] Preferably, in step (3), the copper salt is cupric chloride, cuprous chloride and copper salicylate; and the molar mass of the copper element after the mixture accounts for 1 to 25% of the total molar mass of the metal elements copper, magnesium and aluminum.

[0019] Transition metal salts with empty orbitals can catalyze free radical addition. +It can provide empty orbitals, and it can form more stable free radical transition states with free radicals such as CCl3· and Cl·, reducing the activation energy, so cuprous chloride has a better effect.

[0020] Preferably, in step (3), the modifier is sodium dodecyl sulfate solution, sodium lauryl sulfate solution or sodium dodecyl sulfate solution, more preferably sodium dodecyl sulfate solution; the heating temperature is 200-350°C, and the time is 6-8h; the immersion temperature is 15-25°C, and the time is 12-24h.

[0021] The liquid solubility of copper salt is low. In the original catalyst experiment, organic solvents such as acetonitrile and propionitrile must be used. The solubility can be improved after treatment with the modifier. Sodium dodecyl sulfate has good foaming properties and water solubility, increases the contact area, increases the solubility of the catalyst in the aqueous solution, and is very stable in a wide pH range.

[0022] In a second aspect, the present invention also provides the use of the cation-doped modified MgAl hydrotalcite catalyst obtained by the above preparation method for the polymerization reaction of carbon tetrachloride and vinyl chloride to prepare 1,1,1,3,3-pentachloropropane.

[0023] Preferably, the temperature of the telomerization reaction is 40-110° C. and the time is 3-6 hours.

[0024] Compared with the prior art, the beneficial effects of the present invention are:

[0025] (1) Using MgAl hydrotalcite as the carrier, copper salt was selected for cation doping. 2+ Can replace part of Mg 2+ , which neither changes the layered structure distribution of Mg-Al hydrotalcite nor reduces the influence of the Jiang-Taylor effect of Cu-containing hydrotalcite;

[0026] (2) The catalyst is also modified with sodium dodecyl sulfate to increase its solubility, thereby achieving a higher conversion rate and selectivity in the polymerization of carbon tetrachloride and polyethylene;

[0027] (3) When the catalyst is used for reaction, no co-catalyst or other organic solvents need to be added, and the catalyst can be recycled and reused multiple times, has a high reuse rate, is less polluting, and is safe and environmentally friendly. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with the embodiments.

[0029] Example 1

[0030] 1. Preparation of SDS / Cu / MgAl catalyst

[0031] (1) 7.6923 g of Mg(NO3)2·6H2O and 3.7513 g of Al(NO3)3·9H2O were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution A; 2.88 g of sodium hydroxide and 6.3594 g of sodium carbonate were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution B; 100 mL of deionized water was pre-added in a 1 L round-bottom flask, and the mixed solution A and the mixed solution B were slowly added dropwise, the pH was maintained at 9-10, and the mixture was heated for 15 min to obtain a mixed solution C;

[0032] (2) The mixed solution C was filtered and washed in sequence, and then dried in vacuum at 80° C. for 8 h to obtain a MgAl hydrotalcite catalyst;

[0033] (3) Weighing CuCl powder, thoroughly mixing the CuCl powder with a MgAl hydrotalcite catalyst (the molar mass ratio of Cu element to metal elements Cu, Mg, and Al is 1%), heating at 300° C. for 8 h; filtering the resulting precipitate, washing it three times with ethanol, and drying it at 60° C. for 12 h; dissolving 0.0721 g of sodium dodecyl sulfate in 5 mL of deionized water to obtain a sodium dodecyl sulfate solution with a concentration of 0.05 mol / L, taking 1 g of the dried product, soaking it in the sodium dodecyl sulfate solution for 24 h, filtering and washing it multiple times, washing it, and drying it to obtain a SDS / Cu / MgAl catalyst.

[0034] 2. Application

[0035] Take 0.1g SDS / Cu / MgAl catalyst and add it into the reaction kettle, add 14.767g carbon tetrachloride into the autoclave and seal it. After ensuring that the autoclave does not leak, evacuate the autoclave to replace the air, heat it to 70°C, introduce 2g of vinyl chloride, continue to heat it to 110°C, maintain the pressure in the autoclave at 0.3MPa, react for 5h, and after the reaction is completed, cool it down, vent it, release the pressure, and discharge it to obtain 1,1,1,3,3-pentachloropropane.

[0036] Example 2

[0037] 1. Preparation of SDS / Cu / MgAl catalyst

[0038] (1) 7.6923 g of Mg(NO3)2·6H2O and 3.7513 g of Al(NO3)3·9H2O were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution A; 2.88 g of sodium hydroxide and 6.3594 g of sodium carbonate were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution B; 100 mL of deionized water was pre-added in a 1 L round-bottom flask, and the mixed solution A and the mixed solution B were slowly added dropwise, the pH was maintained at 9-10, and the mixture was heated for 15 min to obtain a mixed solution C;

[0039] (2) The mixed solution C was filtered and washed in sequence, and then dried in vacuum at 80° C. for 8 h to obtain a MgAl hydrotalcite catalyst;

[0040] (3) Weighing CuCl powder, thoroughly mixing the CuCl powder with a MgAl hydrotalcite catalyst (the molar mass ratio of Cu element to metal elements Cu, Mg, and Al is 5%), heating at 300° C. for 8 h; filtering the resulting precipitate, washing it three times with ethanol, and drying it at 60° C. for 12 h; dissolving 0.0721 g of sodium dodecyl sulfate in 5 mL of deionized water to obtain a sodium dodecyl sulfate solution with a concentration of 0.05 mol / L, taking 1 g of the dried product, soaking it in the sodium dodecyl sulfate solution for 24 h, filtering and washing it multiple times, washing it, and drying it to obtain a SDS / Cu / MgAl catalyst.

[0041] 2. Application

[0042] Take 0.1g SDS / Cu / MgAl catalyst and add it into the reaction kettle, add 14.767g carbon tetrachloride into the autoclave and seal it. After ensuring that the autoclave does not leak, evacuate the autoclave to replace the air, heat it to 70°C, introduce 2g of vinyl chloride, continue to heat it to 110°C, maintain the pressure in the autoclave at 0.3MPa, react for 5h, and after the reaction is completed, cool it down, vent it, release the pressure, and discharge it to obtain 1,1,1,3,3-pentachloropropane.

[0043] Example 3

[0044] 1. Preparation of SDS / Cu / MgAl catalyst

[0045] (1) 7.6923 g of Mg(NO3)2·6H2O and 3.7513 g of Al(NO3)3·9H2O were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution A; 2.88 g of sodium hydroxide and 6.3594 g of sodium carbonate were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution B; 100 mL of deionized water was pre-added in a 1 L round-bottom flask, and the mixed solution A and the mixed solution B were slowly added dropwise, the pH was maintained at 9-10, and the mixture was heated for 15 min to obtain a mixed solution C;

[0046] (2) The mixed solution C was filtered and washed in sequence, and then dried in vacuum at 80° C. for 8 h to obtain a MgAl hydrotalcite catalyst;

[0047] (3) Weighing CuCl powder, thoroughly mixing the CuCl powder with a MgAl hydrotalcite catalyst (the molar mass ratio of Cu element to metal elements Cu, Mg, and Al is 10%), heating at 300° C. for 8 h; filtering the resulting precipitate, washing it three times with ethanol, and drying it at 60° C. for 12 h; dissolving 0.0721 g of sodium dodecyl sulfate in 5 mL of deionized water to obtain a sodium dodecyl sulfate solution with a concentration of 0.05 mol / L, taking 1 g of the dried product, soaking it in the sodium dodecyl sulfate solution for 24 h, filtering and washing it multiple times, washing it, and drying it to obtain a SDS / Cu / MgAl catalyst.

[0048] 2. Application

[0049] Take 0.1g SDS / Cu / MgAl catalyst and add it into the reaction kettle, add 14.767g carbon tetrachloride into the autoclave and seal it. After ensuring that the autoclave does not leak, evacuate the autoclave to replace the air, heat it to 70°C, introduce 2g of vinyl chloride, continue to heat it to 110°C, maintain the pressure in the autoclave at 0.3MPa, react for 5h, and after the reaction is completed, cool it down, vent it, release the pressure, and discharge it to obtain 1,1,1,3,3-pentachloropropane.

[0050] Example 4

[0051] 1. Preparation of SDS / Cu / MgAl catalyst

[0052] (1) 7.6923 g of Mg(NO3)2·6H2O and 3.7513 g of Al(NO3)3·9H2O were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution A; 2.88 g of sodium hydroxide and 6.3594 g of sodium carbonate were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution B; 100 mL of deionized water was pre-added in a 1 L round-bottom flask, and the mixed solution A and the mixed solution B were slowly added dropwise, the pH was maintained at 9-10, and the mixture was heated for 15 min to obtain a mixed solution C;

[0053] (2) The mixed solution C was filtered and washed in sequence, and then dried in vacuum at 80° C. for 8 h to obtain a MgAl hydrotalcite catalyst;

[0054] (3) Weighing CuCl powder, thoroughly mixing the CuCl powder with a MgAl hydrotalcite catalyst (the molar mass ratio of Cu element to metal elements Cu, Mg, and Al is 15%), heating at 300° C. for 8 h; filtering the resulting precipitate, washing it three times with ethanol, and drying it at 60° C. for 12 h; dissolving 0.0721 g of sodium dodecyl sulfate in 5 mL of deionized water to obtain a sodium dodecyl sulfate solution with a concentration of 0.05 mol / L, taking 1 g of the dried product, soaking it in the sodium dodecyl sulfate solution for 24 h, filtering and washing it multiple times, washing it, and drying it to obtain a SDS / Cu / MgAl catalyst.

[0055] 2. Application

[0056] Take 0.1g SDS / Cu / MgAl catalyst and add it into the reaction kettle, add 14.767g carbon tetrachloride into the autoclave and seal it. After ensuring that the autoclave does not leak, evacuate the autoclave to replace the air, heat it to 70°C, introduce 2g of vinyl chloride, continue to heat it to 110°C, maintain the pressure in the autoclave at 0.3MPa, react for 5h, and after the reaction is completed, cool it down, vent it, release the pressure, and discharge it to obtain 1,1,1,3,3-pentachloropropane.

[0057] Example 5

[0058] 1. Preparation of SDS / Cu / MgAl catalyst

[0059] (1) 7.6923 g of Mg(NO3)2·6H2O and 3.7513 g of Al(NO3)3·9H2O were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution A; 2.88 g of sodium hydroxide and 6.3594 g of sodium carbonate were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution B; 100 mL of deionized water was pre-added in a 1 L round-bottom flask, and the mixed solution A and the mixed solution B were slowly added dropwise, the pH was maintained at 9-10, and the mixture was heated for 15 min to obtain a mixed solution C;

[0060] (2) The mixed solution C was filtered and washed in sequence, and then dried in vacuum at 80° C. for 8 h to obtain a MgAl hydrotalcite catalyst;

[0061] (3) Weighing CuCl powder, thoroughly mixing the CuCl powder with a MgAl hydrotalcite catalyst (the molar mass ratio of Cu element to metal elements Cu, Mg, and Al is 20%), heating at 300° C. for 8 h; filtering the resulting precipitate, washing it three times with ethanol, and drying it at 60° C. for 12 h; dissolving 0.0721 g of sodium dodecyl sulfate in 5 mL of deionized water to obtain a sodium dodecyl sulfate solution with a concentration of 0.05 mol / L, taking 1 g of the dried product, soaking it in the sodium dodecyl sulfate solution for 24 h, filtering and washing it multiple times, washing it, and drying it to obtain a SDS / Cu / MgAl catalyst.

[0062] 2. Application

[0063] Take 0.1g SDS / Cu / MgAl catalyst and add it into the reaction kettle, add 14.767g carbon tetrachloride into the autoclave and seal it. After ensuring that the autoclave does not leak, evacuate the autoclave to replace the air, heat it to 70°C, introduce 2g of vinyl chloride, continue to heat it to 110°C, maintain the pressure in the autoclave at 0.3MPa, react for 5h, and after the reaction is completed, cool it down, vent it, release the pressure, and discharge it to obtain 1,1,1,3,3-pentachloropropane.

[0064] Example 6

[0065] 1. Preparation of SDS / Cu / MgAl catalyst

[0066] (1) 7.6923 g of Mg(NO3)2·6H2O and 3.7513 g of Al(NO3)3·9H2O were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution A; 2.88 g of sodium hydroxide and 6.3594 g of sodium carbonate were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution B; 100 mL of deionized water was pre-added in a 1 L round-bottom flask, and the mixed solution A and the mixed solution B were slowly added dropwise, the pH was maintained at 9-10, and the mixture was heated for 15 min to obtain a mixed solution C;

[0067] (2) The mixed solution C was filtered and washed in sequence, and then dried in vacuum at 80° C. for 8 h to obtain a MgAl hydrotalcite catalyst;

[0068] (3) Weighing CuCl powder, thoroughly mixing the CuCl powder with a MgAl hydrotalcite catalyst (the molar mass ratio of Cu element to metal elements Cu, Mg, and Al is 25%), heating at 300° C. for 8 h; filtering the resulting precipitate, washing it three times with ethanol, and drying it at 60° C. for 12 h; dissolving 0.0721 g of sodium dodecyl sulfate in 5 mL of deionized water to obtain a sodium dodecyl sulfate solution with a concentration of 0.05 mol / L, taking 1 g of the dried product, soaking it in the sodium dodecyl sulfate solution for 24 h, filtering and washing it multiple times, washing it, and drying it to obtain a SDS / Cu / MgAl catalyst.

[0069] 2. Application

[0070] Take 0.1g SDS / Cu / MgAl catalyst and add it into the reaction kettle, add 14.767g carbon tetrachloride into the autoclave and seal it. After ensuring that the autoclave does not leak, evacuate the autoclave to replace the air, heat it to 70°C, introduce 2g of vinyl chloride, continue to heat it to 110°C, maintain the pressure in the autoclave at 0.3MPa, react for 5h, and after the reaction is completed, cool it down, vent it, release the pressure, and discharge it to obtain 1,1,1,3,3-pentachloropropane.

[0071] Example 7

[0072] 1. Preparation of SDS / Cu / MgAl catalyst

[0073] (1) 7.6923 g of Mg(NO3)2·6H2O and 3.7513 g of Al(NO3)3·9H2O were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution A; 2.88 g of sodium hydroxide and 6.3594 g of sodium carbonate were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution B; 100 mL of deionized water was pre-added in a 1 L round-bottom flask, and the mixed solution A and the mixed solution B were slowly added dropwise, the pH was maintained at 9-10, and the mixture was heated for 15 min to obtain a mixed solution C;

[0074] (2) The mixed solution C was filtered and washed in sequence, and then dried in vacuum at 80° C. for 8 h to obtain a MgAl hydrotalcite catalyst;

[0075] (3) Weigh copper salicylate powder, mix the copper salicylate powder with MgAl hydrotalcite catalyst (the molar mass ratio of Cu element to metal elements Cu, Mg, and Al is 5%), heat at 300° C. for 8 h; filter the resulting precipitate, wash it 3 times with ethanol, and dry it at 60° C. for 12 h; dissolve 0.0721 g of sodium dodecyl sulfate in 5 mL of deionized water to obtain a sodium dodecyl sulfate solution with a concentration of 0.05 mol / L, take 1 g of the dried product and soak it in the sodium dodecyl sulfate solution for 24 h, filter and wash it multiple times, wash and dry it to obtain SDS / Cu / MgAl catalyst.

[0076] 2. Application

[0077] Take 0.1g SDS / Cu / MgAl catalyst and add it into the reaction kettle, add 14.767g carbon tetrachloride into the autoclave and seal it. After ensuring that the autoclave does not leak, evacuate the autoclave to replace the air, heat it to 70°C, introduce 2g of vinyl chloride, continue to heat it to 110°C, maintain the pressure in the autoclave at 0.3MPa, react for 5h, and after the reaction is completed, cool it down, vent it, release the pressure, and discharge it to obtain 1,1,1,3,3-pentachloropropane.

[0078] Example 8

[0079] 1. Preparation of SDS / Cu / MgAl catalyst

[0080] (1) 7.6923 g of Mg(NO3)2·6H2O and 3.7513 g of Al(NO3)3·9H2O were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution A; 2.88 g of sodium hydroxide and 6.3594 g of sodium carbonate were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution B; 100 mL of deionized water was pre-added in a 1 L round-bottom flask, and the mixed solution A and the mixed solution B were slowly added dropwise, the pH was maintained at 9-10, and the mixture was heated for 15 min to obtain a mixed solution C;

[0081] (2) The mixed solution C was filtered and washed in sequence, and then dried in vacuum at 80° C. for 8 h to obtain a MgAl hydrotalcite catalyst;

[0082] (3) Weigh CuCl2 powder, mix the CuCl2 powder with MgAl hydrotalcite catalyst (the molar mass ratio of Cu element to metal elements Cu, Mg, and Al is 5%), and heat at 300°C for 8 hours; wash the precipitate obtained after filtration with ethanol three times and dry it at 60°C for 12 hours; dissolve 0.0721 g of sodium dodecyl sulfate in 5 mL of deionized water to obtain a sodium dodecyl sulfate solution with a concentration of 0.05 mol / L, take 1 g of the dried product and soak it in the sodium dodecyl sulfate solution for 24 hours, filter and wash it multiple times, wash and dry it to obtain SDS / Cu / MgAl catalyst.

[0083] 2. Application

[0084] Take 0.1g SDS / Cu / MgAl catalyst and add it into the reaction kettle, add 14.767g carbon tetrachloride into the autoclave and seal it. After ensuring that the autoclave does not leak, evacuate the autoclave to replace the air, heat it to 70°C, introduce 2g of vinyl chloride, continue to heat it to 110°C, maintain the pressure in the autoclave at 0.3MPa, react for 5h, and after the reaction is completed, cool it down, vent it, release the pressure, and discharge it to obtain 1,1,1,3,3-pentachloropropane.

[0085] Example 9

[0086] 1. Preparation of SDS / Cu / MgAl catalyst

[0087] (1) Weigh 2.5641 g of Mg(NO3)2·6H2O and 3.7513 g of Al(NO3)3·9H2O and dissolve them in 100 mL of deionized water to obtain a mixed solution A; weigh 1.44 g of sodium hydroxide and 2.1198 g of sodium carbonate and dissolve them in 100 mL of deionized water to obtain a mixed solution B; add 100 mL of deionized water to a 1 L round-bottom flask in advance, slowly dropwise add the mixed solution A and the mixed solution B, keep the pH at 9-10, and heat the reaction for 15 min to obtain a mixed solution C;

[0088] (2) The mixed solution C was filtered and washed in sequence, and then dried in vacuum at 80° C. for 8 h to obtain a MgAl hydrotalcite catalyst;

[0089] (3) Weighing CuCl powder, thoroughly mixing the CuCl powder with a MgAl hydrotalcite catalyst (the molar mass ratio of Cu element to metal elements Cu, Mg, and Al is 5%), heating at 300° C. for 8 h; filtering the resulting precipitate, washing it three times with ethanol, and drying it at 60° C. for 12 h; dissolving 0.0721 g of sodium dodecyl sulfate in 5 mL of deionized water to obtain a sodium dodecyl sulfate solution with a concentration of 0.05 mol / L, taking 1 g of the dried product, soaking it in the sodium dodecyl sulfate solution for 24 h, filtering and washing it multiple times, washing it, and drying it to obtain a SDS / Cu / MgAl catalyst.

[0090] 2. Application

[0091] Take 0.1g SDS / Cu / MgAl catalyst and add it into the reaction kettle, add 14.767g carbon tetrachloride into the autoclave and seal it. After ensuring that the autoclave does not leak, evacuate the autoclave to replace the air, heat it to 70°C, introduce 2g of vinyl chloride, continue to heat it to 110°C, maintain the pressure in the autoclave at 0.3MPa, react for 5h, and after the reaction is completed, cool it down, vent it, release the pressure, and discharge it to obtain 1,1,1,3,3-pentachloropropane.

[0092] Comparative Example 1

[0093] The difference from Example 2 is that copper doping is not performed.

[0094] 1. Preparation of SDS / MgAl catalyst

[0095] (1) 7.6923 g of Mg(NO3)2·6H2O and 3.7513 g of Al(NO3)3·9H2O were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution A; 2.88 g of sodium hydroxide and 6.3594 g of sodium carbonate were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution B; 100 mL of deionized water was pre-added in a 1 L round-bottom flask, and the mixed solution A and the mixed solution B were slowly added dropwise, the pH was maintained at 9-10, and the mixture was heated for 15 min to obtain a mixed solution C;

[0096] (2) The mixed solution C was filtered and washed in sequence, and then dried in vacuum at 80° C. for 8 h to obtain a MgAl hydrotalcite catalyst;

[0097] (3) 0.0721 g of sodium dodecyl sulfate was dissolved in 5 mL of deionized water to obtain a sodium dodecyl sulfate solution with a concentration of 0.05 mol / L. 1 g of MgAl hydrotalcite catalyst was placed in the sodium dodecyl sulfate solution and soaked for 24 h. The catalyst was filtered and washed several times, washed and dried to obtain SDS / MgAl catalyst.

[0098] 2. Application

[0099] Take 0.1g SDS / MgAl catalyst and add it to the reactor, add 14.767g carbon tetrachloride into the autoclave and seal it. After ensuring that the autoclave does not leak, evacuate the autoclave to replace the air, heat it to 70°C, introduce 2g of vinyl chloride, continue to heat it to 110°C, maintain the pressure in the autoclave at 0.3MPa, react for 5h, and after the reaction is completed, cool it down, vent it, release the pressure, and discharge it to obtain 1,1,1,3,3-pentachloropropane.

[0100] Comparative Example 2

[0101] The difference from Example 2 is that a SDS / Cu / ZnAl catalyst is prepared.

[0102] 1. Preparation of SDS / Cu / ZnAl catalyst

[0103] (1) 8.9244 g Zn(NO3)2·6H2O and 3.7513 g Al(NO3)3·9H2O were weighed and dissolved in 100 mL deionized water to obtain a mixed solution A; 2.88 g sodium hydroxide and 6.3594 g sodium carbonate were weighed and dissolved in 100 mL deionized water to obtain a mixed solution B; 100 mL deionized water was pre-added in a 1 L round-bottom flask, and the mixed solution A and the mixed solution B were slowly added dropwise, the pH was maintained at 9-10, and the mixture was heated for 15 min to obtain a mixed solution C;

[0104] (2) The mixed solution C was filtered and washed in sequence, and then dried in vacuum at 80° C. for 8 h to obtain a ZnAl hydrotalcite catalyst;

[0105] (3) Weigh CuCl powder, mix the CuCl powder with a ZnAl hydrotalcite catalyst (the molar mass ratio of Cu element to metal elements Cu, Mg, and Al is 5%), and heat at 300° C. for 8 h. After filtering, the resulting precipitate is washed three times with ethanol and dried at 60° C. for 12 h. Dissolve 0.0721 g of sodium dodecyl sulfate in 5 mL of deionized water to obtain a sodium dodecyl sulfate solution with a concentration of 0.05 mol / L. Take 1 g of the dried product and soak it in the sodium dodecyl sulfate solution for 24 h, filter and wash it multiple times, wash and dry it to obtain a SDS / Cu / ZnAl catalyst.

[0106] 2. Application

[0107] Take 0.1g SDS / Cu / ZnAl catalyst and add it into the reaction kettle, add 14.767g carbon tetrachloride into the autoclave and seal it. After ensuring that the autoclave does not leak, evacuate the autoclave to replace the air, heat it to 70°C, introduce 2g of vinyl chloride, continue to heat it to 110°C, maintain the pressure in the autoclave at 0.3MPa, react for 5h, and after the reaction is completed, cool it down, vent it, release the pressure, and discharge it to obtain 1,1,1,3,3-pentachloropropane.

[0108] Comparative Example 3

[0109] The difference from Example 2 is that: a SDS / CuMgAl catalyst is prepared.

[0110] 1. Preparation of SDS / CuMgAl catalyst

[0111] (1) 2.4160 g of Cu(NO3)2·3H2O, 7.6923 g of Mg(NO3)2·6H2O, and 3.7513 g of Al(NO3)3·9H2O were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution A; 3.6 g of sodium hydroxide and 8.4792 g of sodium carbonate were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution B; 100 mL of deionized water was pre-added in a 1 L round-bottom flask, and the mixed solution A and the mixed solution B were slowly added dropwise, the pH was maintained at 9-10, and the mixture was heated for 15 min to obtain a mixed solution C;

[0112] (2) The mixed solution C was filtered and washed in sequence, and then vacuum dried at 80°C for 8 h to obtain a CuMgAl hydrotalcite catalyst; (3) 0.0721 g of sodium dodecyl sulfate was dissolved in 5 mL of deionized water to obtain a sodium dodecyl sulfate solution with a concentration of 0.05 mol / L. 1 g of the dried solution was soaked in the sodium dodecyl sulfate solution for 24 h, filtered and washed multiple times, washed and dried to obtain a SDS / CuMgAl catalyst.

[0113] 2. Application

[0114] Take 0.1g SDS / CuMgAl catalyst and add it into the reaction kettle, add 14.767g carbon tetrachloride into the autoclave and seal it. After ensuring that the autoclave does not leak, evacuate the autoclave to replace the air, heat it to 70°C, introduce 2g of vinyl chloride, continue to heat it to 110°C, maintain the pressure in the autoclave at 0.3MPa, react for 5h, and after the reaction is completed, cool it down, vent it, release the pressure, and discharge it to obtain 1,1,1,3,3-pentachloropropane.

[0115] Comparative Example 4

[0116] The difference from Example 2 is that no modification with a modifier is performed.

[0117] 1. Preparation of Cu / MgAl catalyst

[0118] (1) 7.6923 g of Mg(NO3)2·6H2O and 3.7513 g of Al(NO3)3·9H2O were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution A; 2.88 g of sodium hydroxide and 6.3594 g of sodium carbonate were weighed and dissolved in 100 mL of deionized water to obtain a mixed solution B; 100 mL of deionized water was pre-added in a 1 L round-bottom flask, and the mixed solution A and the mixed solution B were slowly added dropwise, the pH was maintained at 9-10, and the mixture was heated for 15 min to obtain a mixed solution C;

[0119] (2) The mixed solution C was filtered and washed in sequence, and then dried in vacuum at 80° C. for 8 h to obtain a MgAl hydrotalcite catalyst;

[0120] (3) Weighing CuCl powder, thoroughly mixing the CuCl powder with a MgAl hydrotalcite catalyst (the molar mass ratio of Cu element to metal elements Cu, Mg, and Al is 5%), heating at 300° C. for 8 h; filtering the resulting precipitate, washing it three times with ethanol, and drying it at 60° C. for 12 h to obtain a Cu / MgAl catalyst.

[0121] 2. Application

[0122] Take 0.1g Cu / MgAl catalyst and add it into the reaction kettle, add 14.767g carbon tetrachloride into the autoclave and seal it. After ensuring that the autoclave does not leak, evacuate the autoclave to replace the air, heat it to 70°C, introduce 2g of vinyl chloride, continue to heat it to 110°C, maintain the pressure in the autoclave at 0.3MPa, react for 5h, and after the reaction is completed, cool it down, vent it, release the pressure, and discharge it to obtain 1,1,1,3,3-pentachloropropane.

[0123] Comparative Example 5

[0124] The difference from Example 2 is that the catalyst is selected as activated carbon supported cuprous chloride

[0125] 1. Preparation of Cu / C catalyst

[0126] (1) Mix 20 mmol of cuprous chloride and 20 mmol of toluene and keep them at 50°C for 3 h under dry nitrogen. Weigh 10 g of activated carbon and store it in a 250 mL vacuum flask. Transfer the mixture of toluene and cuprous chloride to the flask and stir for 2 h. Keep it at 80°C under vacuum for 2 h to remove the toluene and form an activated carbon-supported catalyst.

[0127] 2. Application

[0128] Take 0.1g SDS / Cu / MgAl catalyst and add it into the reaction kettle, add 14.767g carbon tetrachloride into the autoclave and seal it. After ensuring that the autoclave does not leak, evacuate the autoclave to replace the air, heat it to 70°C, introduce 2g of vinyl chloride, continue to heat it to 110°C, maintain the pressure in the autoclave at 0.3MPa, react for 5h, and after the reaction is completed, cool it down, vent it, release the pressure, and discharge it to obtain 1,1,1,3,3-pentachloropropane.

[0129] Table 1 Catalytic effect of catalysts in the process of preparing 1,1,1,3,3-pentachloropropane by telomerization

[0130]

[0131]

[0132] In Table 1, vinyl chloride conversion rate / %=[(mass of vinyl chloride before reaction-mass of vinyl chloride after reaction) / mass of vinyl chloride before reaction]*100%;

[0133] 1,1,1,3,3-pentachloropropane selectivity / %=[(mass of 1,1,1,3,3-pentachloropropane after reaction-mass of 1,1,1,3,3-pentachloropropane before reaction) / (mass of 1,1,1,3,3-pentachloropropane before reaction-mass of 1,1,1,3,3-pentachloropropane after reaction)]*100%; 1,1,1,3,3-pentachloropropane in this formula is the product of the reaction of polyethylene and carbon tetrachloride; catalyst reusability / %=sum[1-(mass of catalyst after reaction / mass of catalyst before reaction)] / number of reactions*100%.

[0134] As shown in Table 1, in combination with Examples 1-9, the cation-doped modified MgAl catalyst of the present invention has a high reaction conversion rate and selectivity. By adjusting the copper ion loading rate, the carbon tetrachloride conversion rate can be 91.32%, and the selectivity of 1,1,1,3,3-pentachloropropane can be 99.97%, so that the activity of the catalyst is significantly improved; the catalyst stability is also significantly improved, and the reusability is maintained at a high level; when the catalyst is used for reaction, there is no need to add a co-catalyst and other organic solvents, which is low in cost, low in pollution, safe and environmentally friendly. In combination with Example 2 and Comparative Example 1 and Comparative Example 3, compared with not performing cation doping and directly using the CuMgAl hydrotalcite catalyst, copper salt is selected for cation doping, Cu 2+ Can replace part of Mg 2+, neither changes the layered structure distribution of magnesium aluminum hydrotalcite, nor reduces the influence of the ginger-Taylor effect of copper-containing hydrotalcite, and can improve the catalytic activity and stability of the reaction. In combination with Example 2 and Comparative Example 2, hydrotalcite carriers of different metals have differences in catalytic activity, and the present invention can achieve a more excellent synergistic catalytic effect between metal ions, and the reaction selectivity of preparing 1,1,1,3,3-pentachloropropane by the polymerization reaction of carbon tetrachloride and vinyl chloride is also higher. In combination with Example 2 and Comparative Example 4, without modification, the solubility and compatibility of the catalyst in the reaction are poor, which is not conducive to exerting a good catalytic effect. In combination with Example 2 and Comparative Example 5, the existing commonly used catalyst precursors have the same active components, but the catalytic activity is significantly reduced.

[0135] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0136] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. An application of a cation-doped modified MgAl hydrotalcite catalyst, characterized in that: The cation-doped modified MgAl hydrotalcite catalyst is used for the telomerization reaction of carbon tetrachloride and vinyl chloride to prepare 1,1,1,3,3-pentachloropropane; The preparation of the cation-doped modified MgAl hydrotalcite catalyst comprises the following steps: (1) dissolving magnesium salt and aluminum salt in water to obtain a mixed solution A; dissolving sodium hydroxide and sodium carbonate in water to obtain a mixed solution B; reacting the mixed solution A and the mixed solution B by a coprecipitation method to obtain a mixed solution C; (2) The mixed solution C is filtered, washed and dried in sequence to obtain a MgAl hydrotalcite catalyst; (3) A copper salt and a MgAl hydrotalcite catalyst are mixed and heated, wherein the copper salt is cuprous chloride, and then immersed in a modifier, wherein the modifier is a sodium dodecyl sulfate solution, and then washed and dried to obtain a cation-doped modified MgAl hydrotalcite catalyst.

2. The use according to claim 1, characterized in that: In step (1), the magnesium salt and aluminum salt are nitrates, chlorates, sulfates or acetates.

3. The use according to claim 1 or 2, characterized in that: In step (1), the molar ratio of the metal elements magnesium and aluminum in the mixed solution A is 3:1; the molar numbers of sodium hydroxide and sodium carbonate in the mixed solution B follow the following formula: n(NaOH)=1.8*(Mg 2+ + Al 3+ ), n(Na2CO3)=2*(Mg 2+ ), where Mg 2+ Represents Mg 2+ The number of moles of Al 3+ Al 3+ The number of moles.

4. The use according to claim 1, characterized in that: In step (1), the coprecipitation method is as follows: the base solution is prepared as an aqueous solution, mixed solution A and mixed solution B are added dropwise, and the pH is maintained at 9-10.

5. The use according to claim 1, characterized in that: In step (2), the drying is vacuum drying, the drying temperature is 60-90° C., and the drying time is 6-10 hours.

6. The use according to claim 1, characterized in that: In step (3), the molar mass of the copper element after mixing accounts for 1-25% of the total molar mass of the metal elements copper, magnesium and aluminum.

7. The use according to claim 1 or 6, characterized in that: In step (3), the heating temperature is 200-350°C for 6-8 hours; the immersion temperature is 15-25°C for 12-24 hours.

8. The use according to claim 1, characterized in that The temperature of the polymerization reaction is 40-110° C. and the time is 3-6 hours.