Spherical tungsten powder for additive manufacturing, preparation method and application
Through the method of removing nickel and iron by sintering and dissolving solution, the problem that fine particle tungsten powder agglomeration is difficult to ensure high-temperature performance is solved, and spherical tungsten powder with a particle size of about 30 microns suitable for additive manufacturing is prepared, which improves the stability and high temperature of the components performance.
Patent Information
- Application Number
- CN202310168605.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-02-25
AI Technical Summary
The existing fine-grained tungsten powder aggregation method is difficult to ensure the high-temperature performance of tungsten and tungsten alloy components, especially in additive manufacturing, it is difficult to prepare spherical tungsten powder of about 30 microns, resulting in defects in printing components.
By mixing tungsten powder, nickel powder and iron powder into ball mill, the material blank is made and sintered in a high-temperature hydrogen atmosphere to form spherical tungsten powder particles, and nickel and iron are removed in the acid solution to obtain spherical tungsten powder with uniform particle size .
It has achieved the preparation of solid spherical tungsten powder with a particle size of about 30 microns, which is suitable for additive manufacturing and stable 3D printing, reducing defects in printed parts and improving the high-temperature performance of tungsten alloy parts.
Smart Images

Figure CN116422876B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of additive manufacturing, and in particular to spherical tungsten powder for additive manufacturing, a preparation method and application thereof. Background Art
[0002] Additive manufacturing technology is a new and revolutionary manufacturing technology in the manufacturing industry. It changes the traditional production mode of cutting raw materials and assembling parts. The designed product is converted into 3D data through CAD software, and then "printed" layer by layer through a specific molding device (3D printer). Different from traditional "subtractive" manufacturing, additive manufacturing technology does not require raw materials and molds, so it can simplify the manufacturing process of products, shorten the product development cycle, improve efficiency and reduce costs.
[0003] Refractory metals are widely used in aerospace and other fields due to their high melting points. For some complex refractory metal parts used under high temperature conditions, additive manufacturing technology is required. Tungsten is an important refractory metal. As the refractory metal with the highest melting point, additive manufacturing of tungsten and tungsten alloys is currently widely studied. However, coarse-grained tungsten powder is difficult to manufacture, especially tungsten powder above 10 microns. Additive manufacturing requires spherical tungsten powder of about 30 microns for normal powder spreading and stable printing. Although the method of agglomerating fine-grained tungsten powder is used to prepare additive manufacturing powder, there are defects such as voids in the powder, and it is difficult to guarantee the performance of tungsten and tungsten alloy parts, especially high-temperature performance. Summary of the invention
[0004] The main purpose of the present invention is to provide a spherical tungsten powder for additive manufacturing, a preparation method and an application thereof, so as to solve the technical problem that it is difficult to ensure the performance of tungsten and tungsten alloy parts when the additive powder is prepared by agglomerating fine-grained tungsten powder.
[0005] To achieve the above object, the present invention provides a method for preparing spherical tungsten powder for additive manufacturing in a first aspect, comprising:
[0006] Tungsten powder, nickel powder and iron powder are mixed and ball-milled to obtain mixed powder, wherein the particle size of the tungsten powder is 1-3 microns, the particle size of the nickel powder is 0.5-3 microns, and the particle size of the iron powder is 0.5-3 microns.
[0007] The mixed powder is granulated and pressed into a shape to obtain a material body.
[0008] The material blank is degreased at 790-810°C and then sintered at 1450-1530°C in a hydrogen atmosphere for 2-4 hours to obtain a rod.
[0009] The rod is added into a dissolving solution to remove iron and nickel in the rod to obtain spherical tungsten powder. The dissolving solution includes an acid solution. The acid solution can dissolve iron and nickel powders but cannot dissolve tungsten.
[0010] According to an embodiment of the present application, in the mixed powder, the mass percentage of tungsten powder is 93-95%, the mass percentage of nickel powder is 3.5-5%, and the mass percentage of iron powder is 1.5-2.1%.
[0011] According to the implementation mode of the present application, after the material blank is degreased at 800° C., it is sintered at 1450-1530° C. in a hydrogen atmosphere for 2-4 hours to obtain a rod.
[0012] According to the embodiment of the present application, in the step of ball-milling the mixture of tungsten powder, nickel powder and iron powder, the ball-milling medium is ethanol, and 1-3% paraffin is added to the ethanol. The ball-milling time is 24-36 hours, the ball-to-material ratio of the ball mill is 4:1, and the material is the sum of tungsten powder, nickel powder and iron powder.
[0013] According to an embodiment of the present application, the step of granulating the mixed powder includes: spray-drying and granulating the mixed powder at a gas temperature of 150-200°C.
[0014] According to the implementation mode of the present application, the mixed powder particles formed by granulation are pressed into a material green body under a pressure of 150-200 MPa, and the material green body is a sphere with a diameter of 20-50 mm or a block with a width of 20-50 mm.
[0015] According to an embodiment of the present application, the dissolving solution also includes hydrogen peroxide, and the acid solution is one or more of hydrochloric acid, sulfuric acid and nitric acid.
[0016] According to an embodiment of the present application, adding the rod to the dissolving solution to remove the iron and nickel in the rod includes:
[0017] The rod is crushed and added into the dissolving solution to dissolve, and then washed with water, neutralized and filtered to obtain the spherical tungsten powder.
[0018] A second aspect of the present invention provides spherical tungsten powder obtained by the above-mentioned preparation method.
[0019] A third aspect of the present invention provides an application of the spherical tungsten powder obtained by the above-mentioned preparation method in additive manufacturing of metal parts.
[0020] In the above-mentioned method for preparing spherical tungsten powder for additive manufacturing, tungsten powder, nickel powder and iron powder are used as raw materials to sinter to obtain rods. During the sintering process, the particle size of the tungsten powder increases to form spherical tungsten powder particles with larger particles, and the nickel powder and iron powder are melted and coated on the surface of the spherical tungsten powder particles. After the nickel powder and iron powder are removed by the dissolving liquid, spherical tungsten powder is obtained. The above-mentioned method for preparing spherical tungsten powder for additive manufacturing has short steps and simple process. The obtained spherical tungsten powder has a solid particle size and a spherical powder shape, which is suitable for powder laying and stable 3D printing of additive manufacturing, and the printed parts have few defects. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0022] Figure 1 is a scanning electron microscope image of a rod according to an embodiment of the present application;
[0023] Figure 2 is a scanning electron microscope image of the spherical powder according to one embodiment of the present application.
[0024] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] It should be noted that all directional indications (such as up, down, etc.) in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.
[0027] In addition, in the present invention, the descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.
[0028] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0029] To achieve the above object, the present invention provides a method for preparing spherical tungsten powder for additive manufacturing in a first aspect, comprising:
[0030] S10: ball-milling tungsten powder, nickel powder and iron powder to obtain mixed powder, wherein the particle size of the tungsten powder is 1-3 microns, the particle size of the nickel powder is 0.5-3 microns, and the particle size of the iron powder is 0.5-3 microns.
[0031] In this step, 1-3 micron tungsten powder, 0.5-3 micron nickel powder, and 0.5-3 micron iron powder can be mixed and ball-milled. During the ball-milling process, the tungsten powder, nickel powder, and iron powder are further crushed to form finer particles, and the tungsten powder, nickel powder, and iron powder are mixed more evenly. 1-3 micron tungsten powder, 0.5-3 micron nickel powder, and 0.5-3 micron iron powder are relatively easy to obtain and have low cost.
[0032] S20: granulating and pressing the mixed powder to obtain a material body.
[0033] In this step, the mixed powder is granulated to form small particles of mixed powder particles, and then pressed into shape, for example, by grinding or cold isostatic pressing, so that the mixed powder particles form a material body with a certain shape. The material body can be spherical, square, cylindrical, etc., and the specific shape is not limited. The volume of the material body is relatively small, and its maximum three-dimensional size is not too large to facilitate calcination. In some embodiments, the maximum size and minimum size of the material body in three dimensions are similar.
[0034] S30: After degreasing the material blank at 790-810° C., sintering it in a hydrogen atmosphere at 1450-1530° C. for 2-4 hours to obtain a rod.
[0035] The melting point of nickel powder is 212° C., the melting point of iron powder is 1538° C., and the melting point of tungsten powder is 3400° C. In this step, during the sintering process, the tungsten grains gradually grow, so the particle size of the tungsten powder gradually increases, forming a relatively regular spherical structure, that is, forming spherical tungsten powder particles.
[0036] Sintering in hydrogen atmosphere at 1450-1530℃ for 2-4 hours, the sintering degree is good, the melting point of nickel powder and iron powder is relatively low, forming a molten state, covering the surface of spherical tungsten powder particles. That is, the rod includes multiple spherical tungsten powder particles, and the adjacent spherical tungsten powder particles are filled with molten iron and nickel.
[0037] If the temperature is too high and the time is too long, a large amount of tungsten, nickel and iron may melt together, destroying the iron and nickel wrapped around the tungsten particles. The subsequent rods are not easy to break, and the tungsten particles are larger and irregular in shape. If the temperature is too low and the time is too short, the tungsten particles may not grow or may not grow to the target range.
[0038] S40: adding the rod into a dissolving solution to remove iron and nickel in the rod to obtain spherical tungsten powder, wherein the dissolving solution includes an acid solution, which can dissolve iron and nickel powders but cannot dissolve tungsten.
[0039] In this step, since the acid solution can dissolve iron and nickel powder but cannot dissolve tungsten, the iron and nickel filled between adjacent spherical tungsten powder particles are removed by the dissolving liquid, thereby obtaining spherical tungsten powder. In order to speed up the dissolution rate, in some embodiments, the rod can be broken, such as by knocking. The rod is broken to obtain a plurality of rod blocks. Then, the plurality of rod blocks are contacted with the acid solution to dissolve the iron and nickel in the rod blocks. Compared with the direct contact of the rod with the acid solution, the contact area of the above method is increased, and the dissolution rate is accelerated.
[0040] In the above-mentioned method for preparing spherical tungsten powder for additive manufacturing, tungsten powder, nickel powder and iron powder are used as raw materials to sinter to obtain rods. During the sintering process, the particle size of the tungsten powder increases to form spherical tungsten powder particles with larger particles, and the nickel powder and iron powder are melted and coated on the surface of the spherical tungsten powder particles. After the nickel powder and iron powder are removed by the dissolving liquid, spherical tungsten powder is obtained. The above-mentioned method for preparing spherical tungsten powder for additive manufacturing has short steps and simple process. The obtained spherical tungsten powder has a solid particle size and a spherical powder shape, which is suitable for additive manufacturing powder laying and stable 3D printing, and the printed parts have few defects. The particle size of the above-mentioned spherical tungsten powder is about 30 microns, specifically 20-40, for example, 25 to 35 microns, such as 32 microns.
[0041] In some embodiments, in the mixed powder, the mass percentage of tungsten powder is 93-95%, the mass percentage of nickel powder is 3.5-5%, and the mass percentage of iron powder is 1.5-2.1%.
[0042] In some embodiments, the material blank is degreased at 800° C. and then sintered at 1450-1530° C. in a hydrogen atmosphere for 2-4 hours to obtain a rod.
[0043] In some embodiments, in the step of ball-milling the mixed tungsten powder, nickel powder and iron powder, the ball-milling medium is ethanol, and 1-3% paraffin is added to the ethanol. The ball-milling time is 24-36 hours, the ball-to-material ratio of the ball mill is 4:1, and the material is the sum of tungsten powder, nickel powder and iron powder.
[0044] In some embodiments, the step of granulating the mixed powder comprises: spray drying the mixed powder at a gas temperature of 150-200° C. to granulate the mixed powder.
[0045] In some embodiments, the mixed powder particles formed by granulation are pressed into a material green body under a pressure of 150-200 MPa, and the material green body is a sphere with a diameter of 20-50 mm or a cube with a width of 20-50 mm.
[0046] In some embodiments, the dissolving liquid further comprises hydrogen peroxide, and the acid solution is one or more of hydrochloric acid, sulfuric acid and nitric acid. The concentrations of the hydrochloric acid, the sulfuric acid and the nitric acid are 30-40%, and the concentration of the hydrogen peroxide is 27-50%. Exemplarily, the volume ratio of the hydrogen peroxide to the acid solution is 1:1.
[0047] In some embodiments, adding the rod to a dissolving solution to remove iron and nickel from the rod comprises:
[0048] The rod is crushed and added into the dissolving solution to dissolve, and then washed with water, neutralized and filtered to obtain the spherical tungsten powder.
[0049] Among them, water washing can remove most of the solution and the nickel ions and iron ions dissolved in the solution. There may be residual H on the surface of the tungsten particles after water washing. + , it can be removed by immersing it in an alkaline solution to neutralize its surface.
[0050] The present invention also provides spherical tungsten powder obtained by the above preparation method.
[0051] The present invention also provides an application of the spherical tungsten powder obtained by the above-mentioned preparation method in additive manufacturing of metal parts.
[0052] The technical solution of the present application is described below in conjunction with specific embodiments.
[0053] Example 1
[0054] S101 ball milling: tungsten powder, nickel powder and iron powder are mixed and ball milled to obtain a mixed powder. The particle size of the tungsten powder is 3 microns, the particle size of the nickel powder is 2 microns, and the particle size of the iron powder is 3 microns. The mixed powder is 93% tungsten + 4.9% nickel + 2.1% iron powder.
[0055] S102 Spray drying: The mixed powder is dried and granulated by using a closed spray drying method with a centrifugal nozzle at a gas temperature of 150°C.
[0056] S103 pressing: Pressed by grinding or cold isostatic pressing, with a pressure of 150MPa, into small cubes with a diameter of 20mm.
[0057] S104 sintering: After degreasing the material body at 800°C, sinter it in a hydrogen atmosphere at 1500°C for 2 hours to obtain a rod.
[0058] S105 dissolution: dissolve the rod in hydrochloric acid and hydrogen peroxide, wash, neutralize and filter to obtain spherical tungsten powder of about 32 microns.
[0059] Example 2
[0060] S101 ball milling: tungsten powder, nickel powder and iron powder are mixed and ball milled to obtain a mixed powder. The particle size of the tungsten powder is 2 microns, the particle size of the nickel powder is 3 microns, and the particle size of the iron powder is 0.5 microns. The mixed powder is 94% tungsten + 4% nickel + 2% iron powder.
[0061] S102 Spray drying: The mixed powder is dried and granulated by using a closed spray drying method with a centrifugal nozzle at a gas temperature of 180°C.
[0062] S103 pressing: Press by grinding or cold isostatic pressing, with a pressure of 180MPa, into small balls or small cubes with a diameter of 30mm.
[0063] S104 sintering: After degreasing the material body at 800°C, sinter it in a hydrogen atmosphere at 1450°C for 4 hours to obtain a rod.
[0064] S105 dissolution: dissolve the rod in nitric acid and hydrogen peroxide, wash, neutralize and filter to obtain spherical tungsten powder of about 30 microns.
[0065] Example 3
[0066] S101 ball milling: tungsten powder, nickel powder and iron powder are mixed and ball milled to obtain a mixed powder. The particle size of the tungsten powder is 1 micron, the particle size of the nickel powder is 0.5 micron, and the particle size of the iron powder is 2 microns. The mixed powder is 95% tungsten + 3.5% nickel + 1.5% iron powder.
[0067] S102 Spray drying: The mixed powder is dried and granulated by using a closed spray drying method and a centrifugal nozzle at a gas temperature of 200°C.
[0068] S103 pressing: Press by grinding or cold isostatic pressing, with a pressure of 200MPa, into small balls or small cubes with a diameter of 20-50mm.
[0069] S104 sintering: After degreasing the material body at 800°C, sinter it in a hydrogen atmosphere at 1530°C for 3 hours to obtain a rod.
[0070] S105 dissolution: dissolve the rod in sulfuric acid and hydrogen peroxide, wash, neutralize and filter to obtain spherical tungsten powder of about 35 microns.
[0071] Comparative Example 1
[0072] The difference from Example 1 is that the sintering temperature in step S104 is 1400°, and the other parameters and steps are the same as Example 1.
[0073] Comparative Example 2
[0074] The difference from Example 2 is that the sintering time in step S104 is 5 hours, and the other parameters and steps are the same as Example 2.
[0075] Comparative Example 3
[0076] The difference from Example 3 is that the sintering time in step S104 is 2.5 hours, and the other parameters and steps are the same as Example 3.
[0077] Test Case
[0078] The rod material in step S104 of Example 1 was tested using a scanning electron microscope. The results are as follows: Figure 1 As shown. Figure 1 It can be seen that the rod includes a plurality of spherical tungsten powder particles, and the space between adjacent spherical tungsten powder particles is filled with molten iron and nickel. The shape of the spherical tungsten powder particles is relatively regular and the particle size is uniform.
[0079] The spherical tungsten powder in step S105 of Example 1 was tested using a scanning electron microscope. The results are as follows: Figure 2 As shown. Figure 2 It can be seen that the surface of the spherical tungsten powder is relatively smooth, the shape is relatively regular, and the particle size is relatively uniform, basically around 32 microns.
[0080] The spherical tungsten powder in step S105 of comparative example 1 was tested using a scanning electron microscope. The spherical tungsten powder had an irregular shape and a relatively dispersed particle size.
[0081] It can be seen that the above-mentioned method for preparing spherical tungsten powder for additive manufacturing can effectively prepare spherical tungsten powder particles with a particle size of about 30 microns. The powder shape is spherical and the particle size is relatively uniform, which is suitable for additive manufacturing powder laying and stable 3D printing.
[0082] The above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing spherical tungsten powder for additive manufacturing, characterized in that: include: Mix tungsten powder, nickel powder and iron powder and ball mill to obtain mixed powder; wherein the particle size of the tungsten powder is 1-3 microns, the particle size of the nickel powder is 0.5-3 microns, and the particle size of the iron powder is 0.5-3 microns; the ball milling medium is ethanol, and 1-3% paraffin is added to the ethanol; the ball milling time is 24-36 hours, the ball-to-material ratio of the ball milling ball is 4:1, and the material is the sum of the tungsten powder, the nickel powder and the iron powder; in the mixed powder, the mass percentage of the tungsten powder is 93-95%, the mass percentage of the nickel powder is 3.5-5%, and the mass percentage of the iron powder is 1.5-2.1%; Granulating and pressing the mixed powder to obtain a material body; After degreasing the material blank at 790-810° C., sintering it in a hydrogen atmosphere at 1450-1530° C. for 2-4 hours to obtain a rod; The rod is added into a dissolving solution to remove iron and nickel in the rod to obtain the spherical tungsten powder, wherein the dissolving solution includes an acid solution, which can dissolve iron and nickel powders but cannot dissolve tungsten; the dissolving solution also includes hydrogen peroxide, and the acid solution is one or more of hydrochloric acid, sulfuric acid and nitric acid; the concentrations of the hydrochloric acid, the sulfuric acid and the nitric acid are 30-40%, the concentration of the hydrogen peroxide is 27-50%, and the volume ratio of the hydrogen peroxide to the acid solution is 1:
1.
2. The preparation method according to claim 1, characterized in that: The material blank is degreased at 800° C. and then sintered at 1450-1530° C. in a hydrogen atmosphere for 2-4 hours to obtain a rod.
3. The preparation method according to claim 1, characterized in that: The step of granulating the mixed powder comprises: spray drying and granulating the mixed powder at a gas temperature of 150-200°C.
4. The preparation method according to claim 3, characterized in that: The mixed powder particles formed by granulation are pressed into a material green body under a pressure of 150-200 MPa. The material green body is a sphere with a diameter of 20-50 mm or a block with a width of 20-50 mm.
5. The preparation method according to claim 1, characterized in that: The step of adding the rod material into a dissolving solution to remove iron and nickel in the rod material comprises: The rod is crushed and added into the dissolving solution to dissolve, and then washed with water, neutralized and filtered to obtain the spherical tungsten powder.
6. A spherical tungsten powder obtained by the preparation method according to any one of claims 1 to 5.
7. Use of the spherical tungsten powder obtained by the preparation method according to any one of claims 1 to 5 in additive manufacturing of metal parts.
Citation Information
Patent Citations
High specific gravity tungsten alloy material and preparation method thereof
CN104313377A
Manufacture method for glomerate sintered-type thermal spraying tungsten powder
CN106216690A
Method for preparing porous tungsten material based on W-Fe-C system corrosion method
CN111020329A
Metal tungsten powder for laser additive manufacturing of tungsten product, tungsten product and preparation methods of metal tungsten powder and tungsten product
CN111922330A
Preparation method of large-particle spherical tungsten powder
CN112091228A