A method for preparing glass ceramics
By improving the raw material composition and process flow of glass ceramics, and using the primary high-temperature sintering method, the production complexity and product quality problems caused by secondary sintering in the existing technology are solved, and the hardness and beauty are taken into account, which is suitable for dental restorations. Preparation of glass ceramics.
Patent Information
- Application Number
- CN202310392357.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-04-13
AI Technical Summary
The existing glass ceramic preparation process requires secondary sintering, resulting in cumbersome production process, interphase stress in the material leads to internal pores, affecting product quality, and it is difficult to meet the aesthetic and mechanical performance requirements of dental restorations at the same time.
SiO2 and CaO are used as main raw materials to form the main crystal phase of β-silicaite. The glass conversion temperature and chemical stability of glass ceramics are improved through Al2O3, MgO/BaO/ZnO is uniformly dispersed, and Li2O/Na2O/K2O is adjusted to regulate the thermal expansion coefficient and High temperature viscosity, realize the preparation of glass ceramics with high temperature sintering, and simplify the process flow.
The glass ceramic preparation without secondary sintering is achieved, the material hardness reaches 150-200MPa, the cutting accuracy is high, the color is similar to the real teeth, and it is suitable for dental restorations, simplifying production processes, and reducing the risk of deformation and non-fitting.
Smart Images

Figure BDA0004176487740000041 
Figure BDA0004176487740000051
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a dental restoration material, in particular to a method for preparing glass ceramics. Background Art
[0002] Glass ceramics are a widely used dental restoration material. Currently, the actual production of glass ceramics generally includes the following processes: (1) mixing and dispersing raw materials; (2) high-temperature melting; (3) water quenching and cooling; (4) cutting into the target shape; (5) high-temperature sintering and crystallization. Among them, high-temperature melting can be regarded as the first heat treatment. After the first heat treatment, the material is easy to cut to obtain the ideal shape. The subsequent high-temperature sintering can be regarded as the second heat treatment, which uses a higher sintering temperature to crystallize the material and increase the hardness of the material.
[0003] On the other hand, by controlling the heating curve and performing gradient sintering during heat treatment, the material can gradually undergo chemical reactions, which can ultimately give the material a satisfactory color effect. Since the temperature range of the primary heat treatment is limited, a gradient temperature change is generally performed during the secondary sintering to give the material a specific color.
[0004] Patent application CN115028364A discloses a method for preparing glass ceramics, which includes a raw material mixing and dispersing step, a melting step, a gas powder step, a spray granulation step, a dry pressing step, a primary sintering step, and a secondary sintering step. The primary sintering step includes: heating the green body to 350-400°C at a heating rate of 2-5°C / min and keeping it warm for 1h, and then heating it to 550-650°C at a heating rate of 10-20°C / min and keeping it warm for 2h to form a lithium metasilicate crystal phase and a crystal nucleus of CaF. The sintering temperature of the secondary sintering step is 800-950°C. The method combines a primary sintering step with a secondary sintering step, wherein a temperature change curve is used during the primary sintering to promote the formation of a lithium metasilicate crystal phase and a crystal nucleus of CaF. After that, the material is further crystallized in the secondary sintering to meet the product use requirements. However, the above preparation process is cumbersome, especially the two-stage sintering with cooling in between, which will cause stress between different phases in the material, easily lead to internal pores, and finally cause defects in the product. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the existing glass ceramic preparation process and provide a method for preparing glass ceramics, which can obtain a product used as a restoration through a single heat treatment, and can be directly used after cutting and polishing without the need for secondary sintering.
[0006] The traditional glass ceramic preparation process requires a secondary sintering process. The hardness of the first sintered material reaches 100MPA. At this time, it can be cut to obtain a rough product of a predetermined shape. After the secondary sintering, the rough product is crystallized at a higher temperature, and the hardness of the material is increased to about 300. At the same time, because of the crystallization at a higher temperature, the material presents color to meet the aesthetic and mechanical properties of the dental restoration to meet medical requirements. If a high-temperature sintering is performed directly, if the cutting conditions are met, the material is required to have a certain toughness and the hardness cannot be too high, but this hardness does not meet the mechanical requirements of actual product use. On the contrary, if the high-temperature sintering meets the mechanical requirements, especially the hardness requirements, it will be difficult to cut and it will be difficult to obtain a perfect restoration structure.
[0007] In order to solve the above contradiction, the inventors start from the improvement of raw materials, select SiO2 and CaO as the main raw materials, the two form the main crystal phase of β-calcium silicate in glass ceramics, on this basis, Al2O3 is used to improve the glass transition temperature and softening point of glass ceramics, so that uniform mixing can be carried out at a higher temperature, and the chemical stability of glass ceramics is improved. MgO / BaO / ZnO mainly plays a fluxing role, so that different powders can be evenly dispersed during the high-temperature melting process, reducing bubbles remaining in the product, and thus improving the chemical stability of the material. The main function of alkali metal oxides Li2O / Na2O / K2O is to reduce the high-temperature viscosity of glass, further reduce the difficulty of mixing raw materials evenly during the high-temperature melting process, reduce the difficulty of mass production, and at the same time be used to adjust the thermal expansion coefficient of glass ceramics. On the basis of the improvement of raw materials, the inventors further explored the processing technology, and by controlling the temperature and time, the material was sintered once to obtain the product, which can be used directly after cutting and polishing, and also meets the use requirements of the restoration, thereby completing the present invention.
[0008] The specific plan is as follows:
[0009] A method for preparing glass ceramics comprises the following steps:
[0010] S1. Weighing and mixing: obtaining basic glass components, mixing the basic glass components uniformly and then degassing to obtain a mixture, wherein the basic glass components include SiO2, CaO, Al2O3, flux, alkali metal oxides and colorants;
[0011] S2, heating and melting the mixed material to obtain molten glass;
[0012] S3, pouring the glass liquid into a mold, and demoulding to obtain a transparent glass block;
[0013] S4, annealing, nucleation and heat treatment the glass block to obtain the glass ceramic.
[0014] Furthermore, in step S1, the mass ratio of SiO2 in the basic glass component is 55-75%, preferably 60-70%, and more preferably 60-65%;
[0015] Preferably, the mass proportion of CaO is 13-22%, more preferably 15-18%;
[0016] Preferably, the mass proportion of Al2O3 is 4 to 12%, more preferably 5 to 10%.
[0017] Furthermore, in step S1, the flux is at least one of MgO, BaO, and ZnO; preferably ZnO and MgO, or ZnO and BaO;
[0018] Preferably, the mass ratio of the flux in the basic glass component is: ZnO is 1-8%, MgO is 1-8%, or, ZnO is 1-8%, BaO is 1-8%; more preferably, the mass ratio of the flux in the basic glass component is: ZnO is 3-5%, MgO is 3-5%, or, ZnO is 3-5%, BaO is 3-5%.
[0019] Further, in step S1, the alkali metal oxide is at least one of Li2O, Na2O, and K2O; preferably, the alkali metal oxide contains Li2O, and the mass content of Li2O is less than 1%; more preferably, the alkali metal oxide consists of the following components in mass content: Li2O 0.001-1%, Na2O 0-8%, and K2O 0-8%.
[0020] Furthermore, in step S1, the mass ratio of the alkali metal oxide in the basic glass component is 1-8%;
[0021] Preferably, the alkali metal oxide is composed of the following components by mass content: Li2O 0-1%, Na2O 0-8%, K2O0-8%, and Na2O and K2O are not 0 at the same time;
[0022] More preferably, the alkali metal oxide consists of the following components in mass content: Li2O 0-1%, Na2O 0-5%, K2O 0-5%, and Na2O and K2O are not 0 at the same time.
[0023] Furthermore, in step S1, the colorant includes V2O5, Tb4O7, Er2O3, Fe2O3, Eu2O3, Pr6O 11 , MnO2, TiO2 or more;
[0024] Preferably, the mass proportion of the colorant in the basic glass component is 0.5-1.5%, preferably 0.7-1.4%, and more preferably 0.8-1.2%.
[0025] Furthermore, in step S2, the heating and melting temperature is 1500-1700°C, preferably 1550-1650°C, and more preferably 1600-1700°C;
[0026] Preferably, the heating and melting time is 60 to 300 min, preferably 120 to 240 min, and more preferably 150 to 180 min.
[0027] Furthermore, in step S4, the annealing temperature is 500-600°C, preferably 530-580°C; more preferably 550-570°C;
[0028] Preferably, the annealing temperature is maintained for 30 to 90 minutes, preferably 40 to 80 minutes, and more preferably 50 to 70 minutes;
[0029] Preferably, the nucleation temperature is 700-900°C, preferably 720-870°C, more preferably 740-840°C;
[0030] Preferably, the temperature of the heat treatment is 1000-1200°C, preferably 1050-1170°C, more preferably 1100-1150°C;
[0031] Preferably, the heat treatment time is 1 to 240 min, preferably 20 to 120 min, and more preferably 40 to 90 min.
[0032] Furthermore, the glass ceramics prepared by the preparation method of the glass ceramics have at least one of the following (1) to (5):
[0033] (1) The amount of β-calcite crystals in the glass-ceramic accounts for 20% to 60% of the total mass;
[0034] (2) The visible light transmittance of the glass ceramic is 25-40%;
[0035] (3) The crystal particles of the glass ceramic are fine and the color is the same as or similar to the color of human real teeth;
[0036] (4) The hardness of the glass ceramic is 150-200 MPa;
[0037] (5) The glass ceramic is cut at a spindle speed of 60,000 rpm and a cutting accuracy of 0.02 mm without edge chipping or sawtooth.
[0038] The present invention also protects the use of the glass ceramic in dental restorations, especially for making at least one of intra-coronal restorations, inlays, onlays, and veneers.
[0039] Beneficial effects:
[0040] In the present invention, the preparation method of the glass ceramic does not require secondary sintering, has a simple production process flow, and has a high controllability coefficient. On the one hand, it shortens the waiting time for "chairside operation", and on the other hand, the restoration will not be deformed or not fit, and has good edge tightness, which has a good prospect for industrial application. DETAILED DESCRIPTION
[0041] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. In the embodiments, if specific techniques or conditions are not indicated, the techniques or conditions described in the literature in this area or the product specifications are carried out. The reagents used or the instruments that are not indicated by the manufacturer are all conventional products that can be obtained commercially. In the following embodiments, if not specifically stated, "%" refers to weight percentage, and parts refer to weight parts.
[0042] Example 1
[0043] A lithium disilicate glass ceramic and a preparation method and application thereof, the specific steps are as follows:
[0044] The ingredients were prepared according to the ingredient list in Table 1. The raw materials were analytically pure, and potassium oxide, sodium oxide and lithium oxide were introduced from potassium carbonate, sodium carbonate and lithium carbonate, respectively.
[0045] The alkali metal oxide can be one or more of potassium oxide, sodium oxide and lithium oxide, which are introduced by potassium carbonate, sodium carbonate and lithium carbonate respectively. The colorant is used in combination, that is, V2O5, Tb4O7 and Er2O3 are mixed in a mass ratio of 1:1:1.
[0046] After mixing, the ingredients were ball milled for 8 hours to mix evenly, degassed in a muffle furnace, and then placed in a high-temperature melting furnace and melted at 1600°C for 2 hours.
[0047] The obtained melt is poured and demolded, annealed at 550°C, nucleated at 740°C / 60min, and heat treated at 1000°C / 2h to obtain the β-calcium silicate glass ceramic.
[0048] Table 1 Raw material usage (weight %)
[0049]
[0050]
[0051] The prepared calcium silicate glass ceramics were tested and found to have fine crystal particles and a hardness of 150MPA-200MPA. When cut under pressure (spindle speed within 60000rmp, cutting accuracy 0.02mm), there was no edge chipping and no serration, and the cutting performance was good.
[0052] Embodiment 2:
[0053] A lithium disilicate glass ceramic and a preparation method and application thereof, the specific steps are as follows:
[0054] The ingredients were prepared according to the ingredient list in Table 1. The raw materials were analytically pure, and potassium oxide, sodium oxide and lithium oxide were introduced from potassium carbonate, sodium carbonate and lithium carbonate respectively. After the ingredients were prepared, they were ball milled for 8 hours to mix evenly and degassed in a muffle furnace. They were placed in a high-temperature melting furnace and melted at 1600°C for 2 hours.
[0055] The obtained melt is poured and demolded, annealed at 550°C, nucleated at 740°C / 60min, and heat treated at 1000°C / 2h to obtain the β-calcium silicate glass ceramic.
[0056] The prepared calcium silicate glass ceramics were tested and found to have fine crystal particles and a hardness of 150MPA-200MPA. When cut under pressure (spindle speed within 60000rmp, cutting accuracy 0.02mm), there was no edge chipping and no serration, and the cutting performance was good.
[0057] Embodiment 3:
[0058] A lithium disilicate glass ceramic and a preparation method and application thereof, the specific steps are as follows:
[0059] The ingredients were prepared according to the ingredient list in Table 1. The raw materials were analytically pure, and potassium oxide, sodium oxide and lithium oxide were introduced from potassium carbonate, sodium carbonate and lithium carbonate respectively. After the ingredients were prepared, they were ball milled for 8 hours to mix evenly and degassed in a muffle furnace. They were placed in a high-temperature melting furnace and melted at 1600°C for 2 hours.
[0060] The obtained melt is poured and demolded, annealed at 550°C, nucleated at 740°C / 60min, and heat treated at 1000°C / 2h to obtain the β-calcium silicate glass ceramic.
[0061] The prepared calcium silicate glass ceramics were tested and found to have fine crystal particles and a hardness of 150MPA-200MPA. When cut under pressure (spindle speed within 60000rmp, cutting accuracy 0.02mm), there was no edge chipping and no serration, and the cutting performance was good.
[0062] Embodiment 4:
[0063] A lithium disilicate glass ceramic and a preparation method and application thereof, the specific steps are as follows:
[0064] The ingredients were prepared according to the ingredient list in Table 1. The raw materials were analytically pure, and potassium oxide, sodium oxide and lithium oxide were introduced from potassium carbonate, sodium carbonate and lithium carbonate respectively. After the ingredients were prepared, they were ball milled for 8 hours to mix evenly and degassed in a muffle furnace. They were placed in a high-temperature melting furnace and melted at 1600°C for 2 hours.
[0065] The obtained melt is poured and demolded, annealed at 550°C, nucleated at 740°C / 60min, and heat treated at 1000°C / 2h to obtain the β-calcium silicate glass ceramic.
[0066] The prepared calcium silicate glass ceramics were tested and found to have fine crystal particles and a hardness of 150MPA-200MPA. When cut under pressure (spindle speed within 60000rmp, cutting accuracy 0.02mm), there was no edge chipping and no serration, and the cutting performance was good.
[0067] Embodiment 5:
[0068] A lithium disilicate glass ceramic and a preparation method and application thereof, the specific steps are as follows:
[0069] The ingredients were prepared according to the ingredient list in Table 1. The raw materials were analytically pure, and potassium oxide, sodium oxide and lithium oxide were introduced from potassium carbonate, sodium carbonate and lithium carbonate respectively. After the ingredients were prepared, they were ball milled for 8 hours to mix evenly and degassed in a muffle furnace. They were placed in a high-temperature melting furnace and melted at 1600°C for 2 hours.
[0070] The obtained melt is poured and demolded, annealed at 550°C, nucleated at 740°C / 60min, and heat treated at 1000°C / 2h to obtain the β-calcium silicate glass ceramic.
[0071] The prepared calcium silicate glass ceramics were tested and found to have fine crystal particles and a hardness of 150MPA-200MPA. When cut under pressure (spindle speed within 60000rmp, cutting accuracy 0.02mm), there was no edge chipping and no serration, and the cutting performance was good.
[0072] Comparative Example 1:
[0073] A lithium disilicate glass ceramic and a preparation method and application thereof, the specific steps are as follows:
[0074] The ingredients were prepared according to the ingredient list in Table 1. The raw materials were analytically pure, and potassium oxide, sodium oxide and lithium oxide were introduced from potassium carbonate, sodium carbonate and lithium carbonate respectively. After the ingredients were prepared, they were ball milled for 8 hours to mix evenly and degassed in a muffle furnace. They were placed in a high-temperature melting furnace and melted at 1700°C for 300 minutes.
[0075] The obtained melt is poured and demolded, annealed at 550°C, nucleated at 740°C / 60min, and heat treated at 1000°C / 2h to obtain the β-calcium silicate glass ceramic.
[0076] The main problem of this comparative example is that the SiO2 content is too high. Therefore, even if the glass is melted at 1700°C for 300 minutes, a uniformly melted glass block cannot be obtained, and the product is a glass block with uneven color.
[0077] Comparative Example 2:
[0078] A lithium disilicate glass ceramic and a preparation method and application thereof, the specific steps are as follows:
[0079] The ingredients were prepared according to the ingredient list in Table 1. The raw materials were analytically pure, and potassium oxide, sodium oxide and lithium oxide were introduced from potassium carbonate, sodium carbonate and lithium carbonate respectively. After the ingredients were prepared, they were ball milled for 8 hours to mix evenly and degassed in a muffle furnace. They were placed in a high-temperature melting furnace and melted at 1600°C for 2 hours.
[0080] The obtained melt is poured and demolded, annealed at 550°C, nucleated at 740°C / 60min, and heat treated at 1000°C / 2h to obtain the β-calcium silicate glass ceramic.
[0081] The main problem of this comparative example is that the content of the colorant is too low, so the color of the molten glass block is too light, and compared with human real teeth, the color cannot meet the aesthetic requirements of dental restorations.
[0082] Comparative Example 3:
[0083] A lithium disilicate glass ceramic and a preparation method and application thereof, the specific steps are as follows:
[0084] The ingredients were prepared according to the ingredient list in Table 1. The raw materials were analytically pure, and potassium oxide, sodium oxide and lithium oxide were introduced from potassium carbonate, sodium carbonate and lithium carbonate respectively. After the ingredients were prepared, they were ball milled for 8 hours to mix evenly and degassed in a muffle furnace. They were placed in a high-temperature melting furnace and melted at 1600°C for 2 hours.
[0085] The obtained melt is poured and demolded, annealed at 550°C, nucleated at 740°C / 60min, and heat treated at 1000°C / 2h to obtain the β-calcium silicate glass ceramic.
[0086] The main problem of this comparative example is that the CaO content is too low. Therefore, the proportion of the generated β-calcium silicate crystal phase is insufficient, resulting in increased glass transparency. The glass transparency is >50%, which cannot meet the aesthetic requirements of dental restorations.
[0087] Comparative Example 4:
[0088] A lithium disilicate glass ceramic and a preparation method and application thereof, the specific steps are as follows:
[0089] The ingredients were prepared according to the ingredient list in Table 1. The raw materials were analytically pure, and potassium oxide, sodium oxide and lithium oxide were introduced from potassium carbonate, sodium carbonate and lithium carbonate respectively. After the ingredients were prepared, they were ball milled for 8 hours to mix evenly and degassed in a muffle furnace. They were placed in a high-temperature melting furnace and melted at 1600°C for 2 hours.
[0090] The obtained melt is poured and demolded, annealed at 550°C, nucleated at 740°C / 60min, and heat treated at 1000°C / 2h to obtain the β-calcium silicate glass ceramic.
[0091] The main problem of this comparative example is that the alkali metal content is too high. Therefore, the softening point of the generated glass is too low, and it deforms and softens during heat treatment. If the heat treatment temperature is lowered, it is not conducive to the formation of β-calcium silicate, and instead it is replaced by impurities such as lithium disilicate and feldspar, which cannot be used as a dental restoration material.
[0092] Comparative Example 5:
[0093] A lithium disilicate glass ceramic and a preparation method and application thereof, the specific steps are as follows:
[0094] The ingredients were prepared according to the ingredient list in Table 1. The raw materials were analytically pure, and potassium oxide, sodium oxide and lithium oxide were introduced from potassium carbonate, sodium carbonate and lithium carbonate respectively. After the ingredients were prepared, they were ball milled for 8 hours to mix evenly and degassed in a muffle furnace. They were placed in a high-temperature melting furnace and melted at 1600°C for 2 hours.
[0095] The obtained melt is poured and demolded, annealed at 550°C, nucleated at 740°C / 60min, and heat treated at 1000°C / 2h to obtain the β-calcium silicate glass ceramic.
[0096] The main problem of this comparative example is that the aluminum oxide content is too low, so the resulting glass transition temperature is too low, and the softening point is too low, and it deforms and softens during heat treatment. If the heat treatment temperature is lowered, β-calcium silicate cannot be formed and cannot be used as a dental restoration material.
[0097] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0098] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0099] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing glass ceramics, Features: The following steps are involved: S1. Weighing and mixing: obtaining basic glass components, mixing the basic glass components uniformly and then degassing to obtain a mixture. The basic glass components include SiO 2 、CaO、Al 2 O 3 , flux, alkali metal oxides and colorants; the mass ratio of SiO2 in the basic glass component is 55-75%; the mass ratio of CaO is 13-22%, and the mass ratio of Al 2 O 3 The mass ratio of ZnO and MgO is 4-12%, the flux is ZnO and MgO, or ZnO and BaO; the mass ratio of the flux in the basic glass component is: ZnO is 1-8%, MgO is 1-8%, or ZnO is 1-8%, BaO is 1-8%; the alkali metal oxide is composed of the following components by mass: Li 2 O 0.001-1%, Na 2 O0-8%, K 2 O0-8%; the mass ratio of the colorant in the basic glass component is 0.5-1.5%, S2, heating and melting the mixed material to obtain molten glass; S3, pouring the glass liquid into a mold, and demoulding to obtain a transparent glass block; S4, subjecting the glass block to annealing, nucleation and heat treatment to obtain the glass ceramic, wherein the main crystal phase of the glass ceramic is β-calcium siliceous stone.
2. The method for preparing the glass ceramic according to claim 1, Features: In step S1, the SiO 2 The mass ratio is 60-70%.
3. The method for preparing glass ceramics according to claim 2, Features: In step S1, the SiO 2 The mass ratio is 60-65%.
4. The method for preparing glass ceramics according to claim 2, Features: In step S1, the mass ratio of CaO in the basic glass component is 15-18%.
5. The method for preparing glass ceramics according to claim 2, Features: In step S1, Al in the basic glass component 2 O 3 The mass ratio is 5~10%.
6. A method for preparing a glass ceramic according to any one of claims 1 to 5, Features: In step S1, the mass proportion of the flux in the basic glass component is: 3-5% for ZnO, 3-5% for MgO, or 3-5% for ZnO and 3-5% for BaO.
7. A method for preparing a glass ceramic according to any one of claims 1 to 5, Features: In step S1, the mass ratio of the alkali metal oxide in the basic glass component is 1-8%.
8. The method for preparing the glass ceramic according to claim 7, Features: In step S1, the alkali metal oxide Na 2 O and K 2 O is not 0 at the same time.
9. The method for preparing the glass ceramic according to claim 8, Features: In step S1, the alkali metal oxide is composed of the following components by mass: Li 2 O 0.001-1%, Na 2 O 0-5%, K 2 O0-5%, and Na 2 O and K 2 O is not 0 at the same time.
10. A method for preparing the glass ceramic according to any one of claims 1 to 5, Features: In step S1, the colorant includes V 2 O 5 , Tb 4 O 7 , Er 2 O 3 , Fe 2 O 3 、Eu 2 O 3 , Pr 6 O 11 、MnO 2 、TiO 2 One or more of the following.
11. The method for preparing the glass ceramic according to claim 10, Features: In step S1, the mass ratio of the colorant in the basic glass component is 0.7-1.4%.
12. The method for preparing the glass ceramic according to claim 11, Features: In step S1, the mass ratio of the colorant in the basic glass component is 0.8-1.2%.
13. The method for preparing the glass ceramic according to claim 1, Features: In step S2, the heating and melting temperature is 1500-1700°C.
14. The method for preparing the glass ceramic according to claim 13, Features: In step S2, the heating and melting temperature is 1550-1650°C.
15. The method for preparing the glass ceramic according to claim 14, Features: In step S2, the heating and melting temperature is 1600-1700°C.
16. The method for preparing the glass ceramic according to claim 13, Features: In step S2, the heating and melting time is 60 to 300 minutes.
17. The method for preparing the glass ceramic according to claim 16, Features: In step S2, the heating and melting time is 120 to 240 minutes.
18. The method for preparing the glass ceramic according to claim 17, Features: In step S2, the heating and melting time is 150 to 180 minutes.
19. A method for preparing a glass ceramic according to any one of claims 1 or 11-18, Features: In step S4, the annealing temperature is 500-600°C.
20. The method for preparing the glass ceramic according to claim 19, Features: In step S4, the annealing temperature is 530°C to 580°C.
21. The method for preparing the glass ceramic according to claim 20, Features: In step S4, the annealing temperature is 550°C to 570°C.
22. The method for preparing the glass ceramic according to claim 19, Features: In step S4, the annealing temperature is maintained for 30 to 90 minutes.
23. The method for preparing the glass ceramic according to claim 22, Features: In step S4, the annealing temperature is maintained for 40 min to 80 min.
24. The method for preparing the glass ceramic according to claim 23, Features: In step S4, the annealing temperature is maintained for 50 to 70 minutes.
25. The method for preparing the glass ceramic according to claim 19, Features: In step S4, the nucleation temperature is 700-900°C.
26. The method for preparing the glass ceramic according to claim 25, Features: In step S4, the nucleation temperature is 720°C to 870°C.
27. The method for preparing the glass ceramic according to claim 26, Features: In step S4, the nucleation temperature is 740°C to 840°C.
28. The method for preparing the glass ceramic according to claim 19, Features: In step S4, the temperature of the heat treatment is 1000-1200°C.
29. The method for preparing the glass ceramic according to claim 28, Features: In step S4, the temperature of the heat treatment is 1050°C to 1170°C.
30. The method for preparing the glass ceramic according to claim 29, Features: In step S4, the temperature of the heat treatment is 1100°C to 1150°C.
31. The method for preparing the glass ceramic according to claim 19, Features: In step S4, the heat treatment time is 1 to 240 minutes.
32. A method for preparing glass ceramics according to claim 31, Features: In step S4, the heat treatment time is 20 min to 120 min.
33. A method for preparing glass ceramics according to claim 32, Features: In step S4, the heat treatment time is 40 min to 90 min.
34. The glass ceramic prepared by the method for preparing the glass ceramic according to any one of claims 1 to 33, Features: Having at least one of the following (1) to (5): (1) The amount of β-calcite crystals in the glass-ceramic accounts for 20% to 60% of the total mass; (2) The visible light transmittance of the glass ceramic is 25-40%; (3) The crystal particles of the glass ceramic are fine and the color is the same as or similar to the color of human real teeth; (4) The hardness of the glass ceramic is 150-200 MPa; (5) The glass ceramic is cut at a spindle speed of 60,000 rpm and a cutting accuracy of 0.02 mm without edge chipping or sawtooth.
35. Use of the glass ceramic according to claim 34 in dental restorations.
Citation Information
Patent Citations
High-fracture-toughness microcrystalline glass for mobile phone backboard and preparation method of high-fracture-toughness microcrystalline glass
CN112851122A
Lithium disilicate glass ceramic as well as preparation method and application thereof