A single atom hydrogenation catalyst and its preparation method and use
Through the preparation of a single-atom hydrogenation catalyst, the atomic dispersion of defective boron nitride support and active components is solved, and the problems of catalysts are easily deactivated and high temperature and high pressure in the prior art are achieved, and the synthesis of aniline is efficiently catalyzed under low temperature and low pressure. Reduces production costs and by-product generation.
Patent Information
- Application Number
- CN202310353140.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-04-04
AI Technical Summary
In the prior art, the catalytic hydrogenation method of nitrobenzene is prone to deactivate the catalyst in the production of aniline, with frequent side reactions, and requires a variety of metal additives. The preparation process is complex, the safety is low, and the operation is high under high temperature and high pressure, and the cost is high. .
By using the preparation method of a single-atom hydrogenation catalyst, the active component precursor and defective boron nitride support are mixed, and the defective site and alkaline site on the surface of the support are formed through heat treatment, so as to achieve atomic dispersion of the active component. Simplify the preparation process, reduce costs, and achieve efficient catalytic aniline synthesis under low temperature and low pressure.
It significantly improves catalytic activity, reduces by-product generation, reduces production costs, improves the high conversion and selectivity of aniline, avoids catalyst deactivation, and simplifies the process flow.
Smart Images

Figure CN116440936B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst preparation, and relates to a hydrogenation catalyst, in particular to a single-atom hydrogenation catalyst and a preparation method and application thereof. Background Art
[0002] Aniline (AN), also known as aminobenzene in Chinese, is a widely used chemical raw material. Many chemical substances are synthesized from aniline, such as antioxidants and accelerators used in the rubber industry, pigments and dyes, diphenylamine used in plastics, explosives, and petroleum, fungicides and pesticides used in agriculture, analgesics and antipyretics in the pharmaceutical industry, etc. Aniline is mainly used to produce diphenylmethane diisocyanate (MDI), which is then used to make rigid polyurethane foam, which is used as an insulating material for refrigerators and buildings, etc. It can also produce adhesives widely used in the construction industry.
[0003] There are currently three main production processes for aniline, namely, nitrobenzene iron powder reduction method, phenol amination method and nitrobenzene catalytic hydrogenation method. Nitrobenzene iron powder reduction method is the earliest method used for aniline production. The equipment of this method is relatively large, iron powder consumption is high, and a lot of wastewater is generated. At present, this method is gradually being eliminated. The phenol amination method has a simple process, less three wastes, and higher product quality, but this method consumes more energy, has a large infrastructure investment, and has a high overall cost.
[0004] Catalytic hydrogenation of nitrobenzene is the mainstream process for aniline production. Among them, fixed-bed gas-phase catalytic hydrogenation has good maturity and stability, the catalyst and product do not need to be separated, and the equipment cost is low. However, the disadvantage is that the catalyst is easily deactivated during the reaction, the catalyst needs to be replaced frequently, and side reactions are prone to occur when locally overheated. The temperature of nitrobenzene liquid-phase hydrogenation process is lower than that of gas-phase hydrogenation, the production capacity is high, and the by-products are few. The core role is the hydrogenation catalyst. Therefore, the development of efficient and selective catalysts is of great significance to the process of nitrobenzene hydrogenation to produce aniline.
[0005] CN112108139A discloses a platinum-based multi-metal catalyst for synthesizing aniline by liquid-phase hydrogenation of nitrobenzene. The catalyst uses platinum as an active component and two or more of ruthenium, nickel, chromium, lanthanum and tungsten as additives. In the liquid-phase hydrogenation reaction of nitrobenzene, a very high nitrobenzene conversion rate and aniline selectivity can be achieved. However, the catalyst requires multiple metal additives, the preparation process is relatively complicated, and the reaction is carried out at 200°C, which is a high temperature and low safety.
[0006] CN114950532A discloses a catalyst for synthesizing aromatic amines from nitroaromatic compounds and a preparation method thereof. The catalyst uses ruthenium-palladium bimetallic as the catalyst active component and is prepared by impregnation reaction to achieve efficient selective hydrogenation of nitroaromatic compounds. The catalyst utilizes the synergistic effect between ruthenium-palladium bimetallics, uses a large amount of precious metal, and the catalytic effect is affected by the ratio of palladium to ruthenium, and has many preparation steps.
[0007] Therefore, in view of the deficiencies in the prior art, it is necessary to provide a catalyst and a preparation method thereof for efficiently catalyzing the hydrogenation of nitrobenzene to prepare aniline, which can overcome the above-mentioned defects. Summary of the invention
[0008] The object of the present invention is to provide a single-atom hydrogenation catalyst and a preparation method and use thereof. The preparation method of the single-atom hydrogenation catalyst is simple, the dispersion of the active component reaches the atomic level, the catalytic activity is improved, and the synthesis of aniline with high efficiency is achieved under mild conditions, thereby significantly improving the yield.
[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides a method for preparing a single-atom hydrogenation catalyst, the preparation method comprising the following steps:
[0011] (1) mixing an active component precursor and a defective boron nitride carrier to obtain an intermediate mixture;
[0012] (2) The intermediate mixture obtained in step (1) is subjected to heat treatment to obtain the single atom hydrogenation catalyst.
[0013] The single-atom hydrogenation catalyst prepared by the preparation method provided by the present invention has abundant defect sites and alkaline sites on the carrier surface, and the active components are dispersed in single atoms, thereby improving the utilization rate of the active components; at the same time, in the reaction of hydrogenating nitrobenzene to prepare aniline, no alkaline auxiliary agent is introduced, no subsequent separation operation is required, and the production cost is greatly reduced. Under the condition of normal temperature and low pressure, the one-step hydrogenation conversion of nitrobenzene into aniline with high activity and high selectivity is achieved.
[0014] Preferably, the method for preparing the defective boron nitride carrier in step (1) comprises the following steps: mixing boron nitride and a modifier to obtain the defective boron nitride carrier.
[0015] Preferably, the modifier comprises a nitrogen-containing compound and / or a hydroxyl-containing compound.
[0016] Preferably, the nitrogen-containing compound comprises any one of ammonia, urea, ethylenediamine, aniline or naphthylamine, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of urea and ethylenediamine, a combination of aniline and naphthylamine, or a combination of urea, ethylenediamine and aniline.
[0017] Preferably, the hydroxyl-containing compound comprises any one of sodium hydroxide, hydrogen peroxide, potassium hydroxide or lithium hydroxide, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of sodium hydroxide and hydrogen peroxide, a combination of potassium hydroxide and lithium hydroxide, or a combination of sodium hydroxide, hydrogen peroxide, potassium hydroxide and lithium hydroxide.
[0018] Preferably, the mass ratio of the modifier to boron nitride is (5-100):1, for example, 5:1, 20:1, 50:1, 80:1 or 100:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, preferably (10-50):1.
[0019] Preferably, the mixing method comprises ball milling.
[0020] Preferably, the ball mill has a rotation speed of 400-1500 r / min, for example, 400 r / min, 800 r / min, 1000 r / min, 1200 r / min or 1500 r / min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable, preferably 500-1000 r / min.
[0021] Preferably, the ball milling time is 2-50 h, for example, 2 h, 10 h, 20 h, 30 h, 40 h or 50 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, preferably 5-30 h.
[0022] If the ball milling time is too short, the purpose of modification cannot be achieved; if the ball milling time is too long, the coordinated amino sites will be destroyed.
[0023] As a preferred technical solution of the present invention, the boron nitride is prepared by the following method: a boron-containing compound and a nitrogen-containing compound react to obtain the boron nitride.
[0024] Preferably, the reaction temperature is 700-2000°C, for example, 700°C, 1000°C, 1500°C, 1800°C or 2000°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] Preferably, the reaction time is 3-10 h, for example, 3 h, 5 h, 7 h or 10 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] Preferably, the boron-containing compound includes any one of boric acid, borax, boron, sodium metaborate, boron chloride or boron bromide, or a combination of at least two of them. Typical but non-limiting combinations include a combination of boric acid and borax, a combination of boron and sodium metaborate, a combination of boron chloride and boron bromide, or a combination of boric acid, borax, boron and sodium metaborate.
[0027] Preferably, the nitrogen-containing compound comprises any one of cyanamide, dicyandiamide, melamine, thiourea, urea or guanidine hydrochloride, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of cyanamide and dicyandiamide, a combination of melamine and thiourea, a combination of urea and guanidine hydrochloride, or a combination of cyanamide, dicyandiamide, melamine and thiourea.
[0028] Preferably, the molar ratio of the boron-containing compound to the nitrogen-containing compound is 1:(10-30), for example, 1:10, 1:15, 1:20, 1:25 or 1:30, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] Preferably, the active component precursor in step (1) includes any one or a combination of at least two of [Pd(NH3)4](NO3)2, [Pd(NH3)]4SO4, (NH4)2PdCl6, K2PdCl4, Na2PdCl4, Pd(AcAc)2, Pd(OAc)2, PdCl2, Pd(NO3)2, RuCl3·nH2O, Ru2Cl4(CO)6, RuI3, K2RuCl or (NH)4RuCl6. Typical but non-limiting combinations include [Pd(NH3)4](NO3)2 and [Pd(NH3)]4SO4, (NH4)2PdCl6 and K2PdCl4, Na2PdCl4 and Pd(AcAc)2, Pd(OAc)2, PdCl2 and Pd(NO3)2, RuCl3·nH2O and Ru2Cl4(CO)6, or RuI3, K2RuCl and (NH)4RuCl6.
[0030] Preferably, the molar ratio of the active component precursor to the defective boron nitride is (0.01-0.05):1, for example, it can be 0.01:1, 0.02:1, 0.03:1, 0.04:1 or 0.05:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0031] Preferably, the mixing in step (1) comprises ball milling.
[0032] Preferably, the rotation speed of the ball mill is 500-1000 r / min, for example, it can be 500 r / min, 600 r / min, 700 r / min, 800 r / min, 900 r / min or 1000 r / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] Preferably, the ball milling time is 1-15 h, for example, 1 h, 5 h, 8 h, 10 h, 12 h or 15 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] Preferably, the temperature of the heat treatment in step (2) is 100-500°C, for example, 100°C, 200°C, 300°C, 400°C or 500°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0035] Preferably, the heat treatment time in step (2) is 1-12 h, for example, 1 h, 5 h, 8 h, 10 h or 12 h, but is not limited to the listed values. Other values not listed within the numerical range are also applicable, preferably 3-8 h.
[0036] Preferably, the heat treatment in step (2) is performed in an oxygen-free atmosphere.
[0037] Preferably, the gas used for the oxygen-free atmosphere includes any one of nitrogen, hydrogen or argon, or a combination of at least two of them. Typical but non-limiting combinations include a combination of nitrogen and hydrogen, a combination of hydrogen and argon, or a combination of nitrogen, hydrogen and argon.
[0038] In a second aspect, the present invention provides a single-atom hydrogenation catalyst, which is prepared by the preparation method described in the first aspect.
[0039] In a third aspect, the present invention provides a use of the single-atom hydrogenation catalyst as described in the second aspect, wherein the single-atom hydrogenation catalyst is used for hydrogenating nitrobenzene to prepare aniline.
[0040] The single-atom hydrogenation catalyst provided by the present invention can effectively inhibit the generation of by-products dicyclohexylamine and cyclohexylamine without adding an auxiliary agent in the reaction of catalyzing the hydrogenation of nitrobenzene to prepare aniline, thereby reducing the catalyst deactivation caused by the by-products and achieving a high conversion rate of nitrobenzene hydrogenation and a high selectivity for aniline.
[0041] Preferably, the use comprises the following steps: hydrogenating nitrobenzene using a monatomic hydrogenation catalyst under a hydrogen atmosphere.
[0042] Preferably, the mass of the single-atom hydrogenation catalyst is 1-25wt% of the mass of nitrobenzene, for example, it can be 1wt%, 10wt%, 15wt%, 20wt% or 25wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0043] Preferably, the temperature of nitrobenzene hydrogenation is 20-60°C, for example, 20°C, 30°C, 40°C, 50°C or 60°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0044] Preferably, the initial pressure of the nitrobenzene hydrogenation is 0.5-2 MPa, for example, 0.5 MPa, 0.8 MPa, 1 MPa, 1.5 MPa or 2 MPa, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0045] Preferably, the reaction time of the nitrobenzene hydrogenation is 10-60 min, for example, 10 min, 30 min, 40 min, 50 min or 60 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0046] Preferably, the nitrobenzene hydrogenation is carried out in a solvent medium.
[0047] Preferably, the solvent comprises any one of tetrahydrofuran, methanol, isopropanol, ethanol, cyclohexane, cyclohexylamine, n-butanol, toluene, N-methylpyrrolidone or tert-butanol, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of tetrahydrofuran and methanol, a combination of ethanol and cyclohexane, a combination of cyclohexylamine and n-butanol, or a combination of toluene, N-methylpyrrolidone and tert-butanol.
[0048] Compared with the prior art, the present invention has the following beneficial effects:
[0049] (1) The present invention prepares a single-atom hydrogenation catalyst by a simple ball milling and heat treatment method. The single-atom hydrogenation catalyst carrier obtained has a high specific surface area and contains abundant nitrogen active sites, defect sites and basic sites, which can form coordination with the active components, so that the active components are dispersed at the atomic level on the carrier surface, thereby realizing efficient utilization of the active components.
[0050] (2) The nitrogen sites and amino groups of the defective boron nitride carrier simultaneously serve as basic sites to enhance its alkalinity, so that the catalyst can effectively inhibit the formation of by-products dicyclohexylamine and cyclohexylamine without adding additives, reducing the catalyst deactivation caused by by-products. The reaction can be carried out at relatively mild temperature and pressure, achieving a high conversion rate of nitrobenzene hydrogenation and a high selectivity for aniline. Moreover, no alkaline additives are introduced, and no subsequent separation operation is required, which greatly reduces the production cost and reduces the discharge of waste liquid and waste residue. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 It is a transmission electron microscope image of the catalyst obtained in Example 1 of the present invention.
[0052] Figure 2 This is a spherical aberration electron microscope characterization image of the catalyst obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0053] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0054] Example 1
[0055] This embodiment provides a method for preparing a single-atom hydrogenation catalyst, the preparation method comprising the following steps:
[0056] (a) Borax and urea were mixed in a molar ratio of 1:20 and calcined at 900°C for 5 h to obtain hexagonal boron nitride;
[0057] (b) mixing sodium hydroxide and the hexagonal boron nitride obtained in step (a) in a mass ratio of 30:1, dissolving in water, and ball milling at a speed of 700 r / min for 15 h to obtain a mixed solution, centrifuging the mixed solution, filtering, washing until the pH value of the filtrate is 7, and drying the filtrate in a forced air drying oven at 80° C. for 12 h to obtain a defective boron nitride solid;
[0058] (c) mixing the active component precursor [Pd(NH3)4](NO3)2 with the defective boron nitride solid obtained in step (b) at a molar ratio of 0.03:1, and ball milling at a speed of 700 r / min for 10 h to obtain an intermediate mixture;
[0059] (d) The intermediate mixture obtained in step (c) is evenly spread on the surface of a magnetic boat, placed in a tubular furnace, introduced with nitrogen, and calcined at 300°C for 5 h to obtain a single-atom hydrogenation catalyst.
[0060] The transmission electron microscopy image of the catalyst obtained in this example is as follows Figure 1 As shown, the spherical aberration electron microscope characterization diagram is as follows Figure 2 shown. Figure 2The white circle in the figure is metal palladium. It can be seen that the active component metal palladium is dispersed in a single atom on the catalyst surface.
[0061] Example 2
[0062] This embodiment provides a method for preparing a single-atom hydrogenation catalyst, the preparation method comprising the following steps:
[0063] (a) Boric acid and cyanamide are mixed in a molar ratio of 1:10 and calcined at 700°C for 10 h to obtain hexagonal boron nitride;
[0064] (b) mixing urea and the hexagonal boron nitride obtained in step (a) at a mass ratio of 50:1, dissolving in water, and ball milling at a speed of 500 r / min for 30 h to obtain a mixed solution, centrifuging the mixed solution, filtering, washing until the pH value of the filtrate is 7, and placing the filtrate in a forced air drying oven at 80° C. for 12 h to obtain a defective boron nitride solid;
[0065] (c) mixing the active component precursor K2PdCl4 with the defective boron nitride solid obtained in step (b) at a molar ratio of 0.01:1, and ball milling at a speed of 1000 r / min for 1 h to obtain an intermediate mixture;
[0066] (d) The intermediate mixture obtained in step (c) is evenly spread on the surface of a magnetic boat, placed in a tubular furnace, and hydrogen is introduced. The calcination temperature is 100° C. and the calcination time is 8 h to obtain a single-atom hydrogenation catalyst.
[0067] Example 3
[0068] This embodiment provides a method for preparing a single-atom hydrogenation catalyst, the preparation method comprising the following steps:
[0069] (a) Sodium metaborate and thiourea are mixed in a molar ratio of 1:30 and calcined at 2000°C for 3 h to obtain hexagonal boron nitride;
[0070] (b) mixing potassium hydroxide and the hexagonal boron nitride obtained in step (a) at a mass ratio of 10:1, dissolving in water, and ball milling at a speed of 1000 r / min for 5 h to obtain a mixed solution, centrifuging the mixed solution, filtering, washing until the pH value of the filtrate is 7, and placing the filtrate in a forced air drying oven at 80° C. for 12 h to obtain a defective boron nitride solid;
[0071] (c) mixing the active component precursor PdCl2 with the defective boron nitride solid obtained in step (b) at a molar ratio of 0.05:1, and ball milling at a speed of 500 r / min for 15 h to obtain an intermediate mixture;
[0072] (d) The intermediate mixture obtained in step (c) is evenly spread on the surface of a magnetic boat, placed in a tubular furnace, introduced with argon gas, and calcined at a temperature of 500° C. for 3 h to obtain the single-atom hydrogenation catalyst.
[0073] Example 4
[0074] This embodiment provides a method for preparing a single-atom hydrogenation catalyst. Compared with Example 1, the mass ratio of sodium hydroxide to hexagonal boron nitride in step (b) is controlled to be 5:1, and the rest is the same as Example 1.
[0075] Example 5
[0076] This embodiment provides a method for preparing a single-atom hydrogenation catalyst. Compared with Example 1, the mass ratio of sodium hydroxide to hexagonal boron nitride in step (b) is controlled to be 100:1, and the rest is the same as Example 1.
[0077] Example 6
[0078] This embodiment provides a method for preparing a single-atom hydrogenation catalyst. Compared with Example 1, the ball milling speed in step (b) is controlled to be 1500 r / min, the ball milling time is controlled to be 2 h, the calcination time in step (d) is controlled to be 1 h, and the rest is the same as Example 1.
[0079] Example 7
[0080] This embodiment provides a method for preparing a single-atom hydrogenation catalyst. Compared with Example 1, the ball milling speed in step (b) is controlled to be 400 r / min, the ball milling time is controlled to be 50 h, the calcination time in step (d) is controlled to be 12 h, and the rest is the same as Example 1.
[0081] Example 8
[0082] This embodiment provides a method for preparing a single-atom hydrogenation catalyst. Compared with Example 1, the hexagonal boron nitride prepared in step (a) is replaced with commercial boron nitride, and the rest is the same as Example 1.
[0083] Comparative Example 1
[0084] This comparative example provides a method for preparing a hydrogenation catalyst. Compared with Example 1, the hexagonal boron nitride obtained in step (a) is used to replace the defective boron nitride in step (c) to prepare the hydrogenation catalyst, and the defect modification treatment in step (b) is not performed. The rest is the same as Example 1.
[0085] Application Example 1
[0086] This application example provides a method for preparing aniline by hydrogenating nitrobenzene using the single-atom hydrogenation catalyst, the method comprising the following steps:
[0087] 0.123 g of nitrobenzene, 0.01 g of the catalyst prepared in Example 1 and 10 mL of tetrahydrofuran were added to a stainless steel autoclave, and the autoclave was replaced with nitrogen and hydrogen three times respectively, and finally filled with 1 MPa H2. After confirming that it was well sealed, the autoclave was heated to 30°C and kept warm for 50 min. After the reaction was completed, the autoclave was cooled to room temperature with cold water, and after releasing the gas in the autoclave, the autoclave was opened, the catalyst was separated by centrifugation, and the supernatant was taken for gas chromatography analysis. The results are listed in Table 1.
[0088] Application Example 2
[0089] This application example provides a method for preparing aniline by hydrogenating nitrobenzene using the single-atom hydrogenation catalyst, the method comprising the following steps:
[0090] 0.123 g of nitrobenzene, 0.03 g of the catalyst prepared in Example 1 and 10 mL of tetrahydrofuran were added to a stainless steel autoclave, and the autoclave was replaced with nitrogen and hydrogen three times respectively, and finally filled with 0.5 MPa H2. After confirming that it was well sealed, the autoclave was heated to 20°C and kept warm for 60 minutes. After the reaction was completed, the autoclave was cooled to room temperature with cold water, and after releasing the gas in the autoclave, the autoclave was opened, the catalyst was separated by centrifugation, and the supernatant was taken for gas chromatography analysis. The results are listed in Table 1.
[0091] Application Example 3
[0092] This application example provides a method for preparing aniline by hydrogenating nitrobenzene using the single-atom hydrogenation catalyst, the method comprising the following steps:
[0093] 0.123 g of nitrobenzene, 0.001 g of the catalyst prepared in Example 1 and 10 mL of tetrahydrofuran were added to a stainless steel autoclave, and the autoclave was replaced with nitrogen and hydrogen three times respectively, and finally filled with 2 MPa H2. After confirming that it was well sealed, the autoclave was heated to 60°C and kept warm for 10 minutes. After the reaction was completed, the autoclave was cooled to room temperature with cold water, and after releasing the gas in the autoclave, the autoclave was opened, the catalyst was separated by centrifugation, and the supernatant was taken for gas chromatography analysis. The results are listed in Table 1.
[0094] Application Example 4
[0095] This application example provides a method for using the single-atom hydrogenation catalyst to hydrogenate nitrobenzene to prepare aniline. The difference between the method and application example 1 is that the catalyst is replaced with the catalyst prepared in example 2.
[0096] Application Example 5
[0097] This application example provides a method for using the single-atom hydrogenation catalyst to hydrogenate nitrobenzene to prepare aniline. The difference between the method and application example 1 is that the catalyst is replaced with the catalyst prepared in Example 3.
[0098] Application Example 6
[0099] This application example provides a method for using the single-atom hydrogenation catalyst to hydrogenate nitrobenzene to prepare aniline. The difference between the method and application example 1 is that the catalyst is replaced with the catalyst prepared in Example 4.
[0100] Application Example 7
[0101] This application example provides a method for using the single-atom hydrogenation catalyst to hydrogenate nitrobenzene to prepare aniline. The difference between the method and application example 1 is that the catalyst is replaced with the catalyst prepared in Example 5.
[0102] Application Example 8
[0103] This application example provides a method for using the single-atom hydrogenation catalyst to hydrogenate nitrobenzene to prepare aniline. The difference between the method and application example 1 is that the catalyst is replaced with the catalyst prepared in Example 6.
[0104] Application Example 9
[0105] This application example provides a method for using the single-atom hydrogenation catalyst to hydrogenate nitrobenzene to prepare aniline. The difference between the method and application example 1 is that the catalyst is replaced with the catalyst prepared in Example 7.
[0106] Application Example 10
[0107] This application example provides a method for using the single-atom hydrogenation catalyst to hydrogenate nitrobenzene to prepare aniline. The difference between the method and application example 1 is that the catalyst is replaced with the catalyst prepared in Example 8.
[0108] Comparative application example 1
[0109] This comparative application example provides a method for preparing aniline by hydrogenating nitrobenzene using the hydrogenation catalyst. The difference between the method and application example 1 is that the catalyst is replaced by the catalyst prepared in comparative example 1.
[0110] Table 1
[0111]
[0112] From Table 1, we can draw the following conclusions:
[0113] (1) It can be seen from Application Examples 1-5 that the single-atom hydrogenation catalyst obtained by the preparation method of the present invention has excellent catalytic performance, with a nitrobenzene conversion rate of 100% and an aniline selectivity of more than 99%, achieving efficient catalysis of the hydrogenation reaction of nitrobenzene to prepare aniline.
[0114] (2) Application Examples 6-9 also achieved good nitrobenzene conversion rate and aniline selectivity. However, compared with Application Example 1, the mass ratio of the modifier to boron nitride in Application Example 6 was 5:1, and the mass ratio of the modifier to boron nitride in Application Example 7 was 100:1, which exceeded the preferred (10-50):1 of the present invention, resulting in a decrease in catalytic performance and a nitrobenzene conversion rate lower than that of Application Example 1. In Application Example 8, the ball milling speed in step (b) was 1500 r / min, the ball milling time was 2 h, and the calcination time in step (d) was 1 h. In Application Example 9, the ball milling speed in step (b) was 400 r / min, the ball milling time was 50 h, and the calcination time in step (d) was 12 h, which exceeded the preferred ball milling speed of 500-1000 r / min, the ball milling time of 5-30 h, and the preferred calcination time of 3-8 h in step (d) of the present invention, resulting in a decrease in catalytic performance and a nitrobenzene conversion rate lower than that of Application Example 1.
[0115] (3) By comparing Application Example 1 with Application Example 10, it can be seen that the boron nitride used in Application Example 8 is commercial boron nitride, and the conversion rate of nitrobenzene decreases. Therefore, it can be seen that the method for preparing hexagonal boron nitride provided by the present invention can achieve better catalytic effect.
[0116] (4) By comparing Application Example 1 with Comparative Application Example 1, it can be seen that the carrier of the hydrogenation catalyst prepared in Comparative Application Example 1 is hexagonal boron nitride, and no defect treatment is performed. The nitrobenzene conversion rate is greatly reduced. It can be seen that the catalytic effect of using defective boron nitride as a carrier of the hydrogenation catalyst is significantly higher than that of untreated boron nitride. The surface of the defective boron nitride carrier in the single-atom hydrogenation catalyst has abundant defect sites and basic sites, which can form strong coordination with the active components, so that the active components are anchored on the carrier surface in the form of single atoms, realizing efficient utilization of the active components.
[0117] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a single-atom hydrogenation catalyst, characterized in that: The preparation method comprises the following steps: (1) mixing an active component precursor and a defective boron nitride carrier to obtain an intermediate mixture; (2) The intermediate mixture obtained in step (1) is subjected to heat treatment to obtain the single atom hydrogenation catalyst; The method for preparing the defective boron nitride carrier in step (1) comprises the following steps: ball milling boron nitride and a modifier to obtain the defective boron nitride carrier; The mass ratio of the modifier to boron nitride is (10-50):1; The ball milling speed of the ball milling boron nitride and the modifier is 500-1000r / min; The ball milling time of the ball milled boron nitride and the modifier is 5-30h; The modifier includes a nitrogen-containing compound and / or a hydroxyl-containing compound; The nitrogen-containing compound includes any one of urea, ethylenediamine, aniline or naphthylamine, or a combination of at least two thereof; The hydroxyl-containing compound includes any one of sodium hydroxide, hydrogen peroxide, potassium hydroxide or lithium hydroxide, or a combination of at least two thereof.
2. The preparation method according to claim 1, characterized in that: The boron nitride is prepared by the following method: The boron-containing compound and the nitrogen-containing compound react to obtain the boron nitride.
3. The preparation method according to claim 2, characterized in that: The reaction temperature is 700-2000° C. and the reaction time is 3-10 hours.
4. The preparation method according to claim 2, characterized in that: The boron-containing compound includes any one of boric acid, borax, elemental boron, sodium metaborate, boron chloride or boron bromide, or a combination of at least two thereof.
5. The preparation method according to claim 2, characterized in that: The nitrogen-containing compound includes any one of cyanamide, dicyandiamide, melamine, thiourea, urea or guanidine hydrochloride, or a combination of at least two thereof.
6. The preparation method according to claim 2, characterized in that: The molar ratio of the boron-containing compound to the nitrogen-containing compound is 1:(10-30).
7. The preparation method according to claim 1, characterized in that: The active component precursor in step (1) includes any one of [Pd(NH3)4](NO3)2, [Pd(NH3)]4SO4, (NH4)2PdCl6, K2PdCl4, Na2PdCl4, Pd(AcAc)2, Pd(OAc)2, PdCl2, Pd(NO3)2, RuCl3·nH2O, Ru2Cl4(CO)6 or RuI3, or a combination of at least two thereof.
8. The preparation method according to claim 1, characterized in that: The molar ratio of the active component precursor to the defective boron nitride in step (1) is (0.01-0.05):
1.
9. The preparation method according to claim 1, characterized in that: The method of mixing the active component precursor and the defective boron nitride carrier in step (1) includes ball milling.
10. The preparation method according to claim 9, characterized in that: The ball milling speed of the ball milling active component precursor and the defective boron nitride carrier is 500-1000r / min.
11. The preparation method according to claim 9, characterized in that: The ball milling time of the ball milling active component precursor and the defective boron nitride carrier is 1-15 hours.
12. The preparation method according to claim 1, characterized in that: The temperature of the heat treatment in step (2) is 100-500°C.
13. The preparation method according to claim 1, characterized in that: The heat treatment time in step (2) is 1-12 hours.
14. The preparation method according to claim 13, characterized in that: The heat treatment time in step (2) is 3-8 hours.
15. The preparation method according to claim 1, characterized in that: The heat treatment in step (2) is carried out in an oxygen-free atmosphere.
16. The preparation method according to claim 15, characterized in that: The gas used in the oxygen-free atmosphere includes any one of nitrogen, hydrogen or argon, or a combination of at least two of them.
17. A single atom hydrogenation catalyst, characterized in that The single-atom hydrogenation catalyst is prepared by the preparation method described in any one of claims 1-16.
18. Use of the single-atom hydrogenation catalyst as claimed in claim 17, characterized in that: The single-atom hydrogenation catalyst is used for preparing aniline by hydrogenating nitrobenzene.
19. The use according to claim 18, characterized in that The use comprises the following steps: hydrogenating nitrobenzene using a single-atom hydrogenation catalyst under a hydrogen atmosphere.
20. The use according to claim 18, characterized in that The mass of the single-atom hydrogenation catalyst is 1-25wt% of the mass of nitrobenzene.
21. The use according to claim 18, characterized in that The temperature of the nitrobenzene hydrogenation is 20-60°C.
22. The use according to claim 18, characterized in that The initial pressure of the nitrobenzene hydrogenation is 0.5-2MPa.
23. The use according to claim 18, characterized in that The reaction time of the nitrobenzene hydrogenation is 10-60 min.
24. The use according to claim 18, characterized in that The nitrobenzene hydrogenation is carried out in a solvent medium.
25. The use according to claim 24, characterized in that The solvent includes any one of tetrahydrofuran, methanol, isopropanol, ethanol, cyclohexane, cyclohexylamine, n-butanol, toluene, N-methylpyrrolidone or tert-butanol, or a combination of at least two thereof.