A method for synthesizing zirconium carbide aerogel using inorganic zirconium salt and phenolic resin

ZrC aerogel is prepared by the sol-gel method of inorganic zirconium salt and phenolic resin, which solves the problem of easy oxidation of carbide aerogel and realizes ZrC aerogel with low thermal conductivity and high mechanical properties, which is suitable for high-temperature insulation materials. .

CN116443878BInactive Publication Date: 2024-10-11BEIJING INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310386785.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Carbide aerogels are easily oxidized in an aerobic environment, which poses safety risks. Research is limited and there is a lack of cheap and easily available preparation methods.

Method used

Using inorganic zirconium salt, novolac phenolic resin and ethanol as raw materials, C/ZrC aerogel was prepared through sol-gel method and carbothermal reduction reaction. The phenolic/ZrO2 double network gel was used for high-temperature carbothermal reduction to obtain low thermal conductivity and good Mechanical properties of ZrC aerogels.

Benefits of technology

The ZrC aerogel that maintains low thermal conductivity and high mechanical properties at high temperatures is achieved, reducing the risk of oxidation and providing a cheap and easy-to-available preparation method suitable for high-temperature insulation materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116443878B_ABST
    Figure CN116443878B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for synthesizing zirconium carbide aerogel using inorganic zirconium salt and phenolic resin, and belongs to the field of aerogel preparation. The present invention uses inorganic zirconium salt, linear phenolic resin and ethanol as raw materials, and prepares C / ZrC aerogel with low thermal conductivity and good mechanical strength through sol-gel method, normal pressure drying and carbon thermal reduction reaction. The density of the aerogel is 0.24g / cm 3 The thermal conductivity at room temperature and 800°C is 0.06 W·m ‑1 ·K ‑1 and 0.15W·m ‑1 ·K ‑1 , and the compression strength is 3.45MPa. The purpose of the present invention is to provide a method for preparing ZrC aerogel using cheap, easily available, and more easily controllable inorganic salts as raw materials, which can be applied to the field of high-temperature thermal insulation materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for synthesizing zirconium carbide aerogel by using inorganic zirconium salt and phenolic resin, belonging to the field of aerogel preparation. Background Art

[0002] Zirconium carbide aerogel has the advantages of high melting point, high strength, and low thermal conductivity. It is a new type of high-temperature thermal protection material. It can be used as a surface thermal protection material for aircraft that work in the atmospheric environment for a long time and are subjected to severe thermal shock and aerodynamic scouring.

[0003] Aerogel is a material with high porosity and three-dimensional skeleton structure, which makes it have extremely low density and good thermal insulation performance. Carbon aerogel can be used in vacuum and inert environment at 2000℃~3000℃, but it is easily oxidized in oxygen environment, so there are great safety risks when using it. Carbide aerogel has good mechanical strength and good antioxidant properties, which can effectively solve the problem of carbon aerogel being easily oxidized. At present, the research on carbide aerogel mainly focuses on SiC aerogel, and the research on other carbide aerogels is not very extensive. Summary of the invention

[0004] The purpose of the present invention is to provide a method for synthesizing carbonized zirconium aerogel using inorganic zirconium salt and phenolic resin; the present invention uses inorganic zirconium salt, linear phenolic resin and ethanol as raw materials, and prepares C / ZrC aerogel with low thermal conductivity and good mechanical strength by sol-gel method, normal pressure drying and carbon thermal reduction reaction. The density of the aerogel is 0.24g / cm 3 The thermal conductivity at room temperature and 800°C is 0.06 W·m -1 ·K -1 and 0.15W·m -1 ·K -1 , and the compression strength is 3.45MPa. The purpose of the present invention is to provide a method for preparing ZrC aerogel using cheap, easily available, and more easily controllable inorganic salts as raw materials, which can be applied to the field of high-temperature thermal insulation materials.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] A method for synthesizing zirconium carbide aerogel using an inorganic zirconium salt and a phenolic resin comprises the following steps:

[0007] Step 1, preparing ZrO2 sol: dissolving an inorganic zirconium salt in a mixed solution of ethanol and deionized water, stirring to fully dissolve the inorganic zirconium salt, obtaining an inorganic zirconium salt with a concentration of 0.5-2 mol / L, and then sequentially adding an acid catalyst and N,N-dimethylformamide to fully hydrolyze the zirconium salt to obtain ZrO2 sol. The molar ratio of the inorganic zirconium salt, the acid catalyst, and the N,N-dimethylformamide is 1:(0.5-2):(0.5-2);

[0008] Step 2: dissolving the linear phenolic resin in an ethanol solution, wherein the mass fraction of the linear phenolic resin is 5-50wt%, stirring until completely dissolved to obtain a transparent and uniform solution, then adding hexamethylenetetramine as a crosslinking agent, stirring until completely dissolved to obtain a phenolic resin sol. The amount of the crosslinking agent added is 3-10% of the mass of the phenolic resin;

[0009] Step 3: Add the phenolic sol prepared in step 2 to the zirconium dioxide sol prepared in step 1, and stir for a period of time to obtain an organic-inorganic two-component sol.

[0010] Step 4: The organic-inorganic two-component sol of step 3 is subjected to sol-gel reaction in an oven at 80-100°C for 10-72h to obtain a phenolic / ZrO2 double network gel, which is then placed in a 60-150°C forced air drying oven for gradient temperature drying or supercritical drying to obtain a phenolic / ZrO2 double network aerogel.

[0011] Step 5: subjecting the phenolic formaldehyde / ZrO2 double network aerogel in step 4 to high temperature carbon thermal reduction reaction in an inert atmosphere or vacuum condition to obtain ZrC aerogel.

[0012] Furthermore, the inorganic zirconium salt described in step 1 is any one of zirconium oxychloride octahydrate, zirconium oxynitrate, and zirconium tetrachloride.

[0013] Furthermore, the acid catalyst in step 1 is any one of acetic acid, nitric acid and hydrochloric acid.

[0014] Furthermore, the mass ratio of the phenolic sol to the ZrO2 sol in step 3 is 0.5-2:1;

[0015] Furthermore, the temperature of high-temperature carbon thermal reduction of the phenolic / ZrO2 double network aerogel described in step 5 is 800-1600°C;

[0016] Beneficial effects:

[0017] (1) This method uses inorganic zirconium salt as a zirconium source and linear phenolic resin to prepare a phenolic / zirconium dioxide composite aerogel with a double network, and then obtains ZrC aerogel through a high-temperature carbothermal reduction reaction. The carbothermal reduction reaction starts at 1400°C and ends at 1600°C.

[0018] (2) The ZrC aerogel obtained by the method of the present invention maintains low thermal conductivity at high temperatures: the thermal conductivity at room temperature is 0.06 W·m -1 ·K -1 , which is lower than the thermal conductivity of organic zirconium salt as zirconium source, which is 0.09-0.11 W·m -1 ·K -1 The thermal conductivity at high temperatures of 200℃, 400℃, 600℃ and 800℃ is 0.0723W·m -1 ·K -1 ,0.1216W·m -1 ·K -1 ,0.1369W·m -1 ·K -1 and 0.1531 W·m -1 ·K -1 .

[0019] (3) The ZrC aerogel obtained by the method of the present invention is a complete crack-free block with good mechanical properties and a compressive strength of 3.45 MPa. In summary, the method of the present invention proposes a method for preparing ZrC aerogel using cheaper and more readily available inorganic zirconium salts as a zirconium source, and the ZrC aerogel obtained by the method has good high-temperature thermal insulation properties and mechanical properties, which is conducive to the application of ZrC aerogel in the field of high-temperature thermal insulation. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a physical picture of the ZrC aerogel prepared in Example 1;

[0021] Figure 2 The thermal conductivity pictures of the ZrC aerogel prepared in Example 1 at high temperature; wherein, Figure a is a macroscopic image of the ZrC aerogel after being treated at 800°C; Figure b is a trend diagram of thermal conductivity changes at different high temperatures;

[0022] Figure 3 X-ray diffraction images of the ZrC aerogel prepared in Example 1 after heat treatment at different temperatures;

[0023] Figure 4 This is the stress-strain curve of the ZrC aerogel prepared in Example 1. DETAILED DESCRIPTION

[0024] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0025] Example 1

[0026] A method for synthesizing zirconium carbide aerogel using an inorganic zirconium salt and a phenolic resin comprises the following steps:

[0027] Dissolve zirconium oxychloride octahydrate in a mixed solution of ethanol and deionized water, stir for 30 minutes, then add acetic acid and N,N-dimethylformamide in turn and stir for 30 minutes to obtain ZrO2 sol. The molar ratio of zirconium oxychloride octahydrate, acetic acid and N,N-dimethylformamide is 1:1:0.5; dissolve linear phenolic resin in ethanol solution, the concentration of phenolic resin is 5wt%, add hexamethylenetetramine, stir until completely dissolved, and obtain phenolic resin sol. The amount of hexamethylenetetramine added is 5% of the mass of phenolic resin; add phenolic sol to ZrO2 sol, stir for a period of time to obtain transparent sol, wherein the mass ratio of phenolic sol to ZrO2 sol is 1:1, and the above two-component sol is placed in a 100℃ oven for aging for 24 hours to obtain phenolic / ZrO2 double network gel. Then place it in a 60-150℃ blast drying oven for gradient temperature drying to obtain phenolic / ZrO2 double network aerogel. Finally, the phenolic / ZrO2 double network aerogel was placed in a vacuum carbonization furnace and calcined at 1600°C in an argon atmosphere to obtain ZrC aerogel. After characterization, the density of the obtained aerogel was 0.24 g / cm 3 , the room temperature thermal conductivity is 0.0625 W·m -1 ·K -1 , the thermal conductivity can still be maintained at 0.1531 W·m at 800℃ -1 ·K -1 , and the macroscopic morphology is complete. Only ZrC crystal phase was detected in the XRD test, and the compressive strength reached 3.45MPa.

[0028] Example 2

[0029] A method for synthesizing zirconium carbide aerogel using an inorganic zirconium salt and a phenolic resin comprises the following steps:

[0030] Dissolve zirconium oxynitrate in a mixed solution of ethanol and deionized water, stir for 30 minutes, then add nitric acid and N,N-dimethylformamide in turn and stir for 30 minutes to obtain ZrO2 sol. The molar ratio of zirconium oxynitrate, acetic acid and N,N-dimethylformamide is 1:1:0.5; dissolve linear phenolic resin in ethanol solution, the concentration of phenolic resin is 10wt%, add hexamethylenetetramine, stir until completely dissolved, and obtain phenolic resin sol. The amount of hexamethylenetetramine added is 8% of the mass of phenolic resin; add phenolic sol to ZrO2 sol, stir for a period of time to obtain transparent sol, wherein the mass ratio of phenolic sol to ZrO2 sol is 1.5:1, and place the above two-component sol in a 100℃ oven for aging for 24 hours to obtain phenolic / ZrO2 double network gel. Then it is supercritically dried to obtain phenolic / ZrO2 double network aerogel. Finally, the phenolic / ZrO2 double network aerogel was placed in a vacuum carbonization furnace and calcined at 1600°C in an argon atmosphere to obtain ZrC aerogel. After characterization, the density of the obtained aerogel was 0.37 g / cm 3 , the room temperature thermal conductivity is 0.0756 W·m -1 ·K -1 .

[0031] Example 3

[0032] A method for synthesizing zirconium carbide aerogel using an inorganic zirconium salt and a phenolic resin comprises the following steps:

[0033] Dissolve zirconium tetrachloride in a mixed solution of ethanol and deionized water, stir for 30 minutes, then add hydrochloric acid and N,N-dimethylformamide in turn and stir for 30 minutes to obtain ZrO2 sol. The molar ratio of zirconium tetrachloride, acetic acid and N,N-dimethylformamide is 1:1:0.5; dissolve linear phenolic resin in ethanol solution, the concentration of phenolic resin is 15wt%, add hexamethylenetetramine, stir until completely dissolved, and obtain phenolic resin sol. The amount of hexamethylenetetramine added is 3% of the mass of phenolic resin; add phenolic sol to ZrO2 sol, stir for a period of time to obtain transparent sol, wherein the mass ratio of phenolic sol to ZrO2 sol is 1:1, and the above two-component sol is placed in a 100℃ oven for aging for 24 hours to obtain phenolic / ZrO2 double network gel. Then it is supercritically dried to obtain phenolic / ZrO2 double network aerogel. Finally, the phenolic / ZrO2 double network aerogel was placed in a vacuum carbonization furnace and calcined at 1600°C in an argon atmosphere to obtain ZrC aerogel. After characterization, the density of the obtained aerogel was 0.31 g / cm 3 , the room temperature thermal conductivity is 0.0745 W·m -1 ·K -1 .

[0034] Example 4

[0035] A method for synthesizing zirconium carbide aerogel using an inorganic zirconium salt and a phenolic resin comprises the following steps:

[0036] Dissolve zirconium oxychloride octahydrate in a mixed solution of ethanol and deionized water, stir for 30 minutes, then add acetic acid and N,N-dimethylformamide in turn and stir for 30 minutes to obtain ZrO2 sol. The molar ratio of zirconium oxychloride octahydrate, acetic acid and N,N-dimethylformamide is 1:0.5:0.5; dissolve linear phenolic resin in ethanol solution, the concentration of phenolic resin is 5wt%, add hexamethylenetetramine, stir until completely dissolved, and obtain phenolic resin sol. The amount of hexamethylenetetramine added is 5% of the mass of phenolic resin; add phenolic sol to ZrO2 sol, stir for a period of time to obtain transparent sol, wherein the mass ratio of phenolic sol to ZrO2 sol is 1:1, and place the above two-component sol in a 100℃ oven for aging for 24 hours to obtain phenolic / ZrO2 double network gel. Then, it was placed in a 60-150°C forced air drying oven for gradient drying or supercritical drying to obtain phenolic / ZrO2 double network aerogel. Finally, the phenolic / ZrO2 double network aerogel was placed in a vacuum carbonization furnace and calcined at 800°C in an argon atmosphere to obtain ZrC aerogel. After characterization, the density of the obtained aerogel was 0.335 g / cm 3 , the room temperature thermal conductivity is 0.0654 W·m -1 ·K -1 The aerogel calcined at this temperature is still amorphous and has a compressive strength of only 2.10 MPa.

[0037] Example 5

[0038] A method for synthesizing zirconium carbide aerogel using an inorganic zirconium salt and a phenolic resin comprises the following steps:

[0039] Dissolve zirconium oxychloride octahydrate in a mixed solution of ethanol and deionized water, stir for 30 minutes, then add acetic acid and N,N-dimethylformamide in turn and stir for 30 minutes to obtain ZrO2 sol. The molar ratio of zirconium oxychloride octahydrate, acetic acid and N,N-dimethylformamide is 1:1:0.5; dissolve linear phenolic resin in ethanol solution, the concentration of phenolic resin is 5wt%, add hexamethylenetetramine, stir until completely dissolved, and obtain phenolic resin sol. The amount of hexamethylenetetramine added is 5% of the mass of phenolic resin; add phenolic sol to ZrO2 sol, stir for a period of time to obtain transparent sol, wherein the mass ratio of phenolic sol to ZrO2 sol is 1.5:1, and place the above two-component sol in a 100℃ oven for aging for 24 hours to obtain phenolic / ZrO2 double network gel. Then, it was placed in a 60-150°C forced air drying oven for gradient drying or supercritical drying to obtain phenolic / ZrO2 double network aerogel. Finally, the phenolic / ZrO2 double network aerogel was placed in a vacuum carbonization furnace and calcined at 1000°C in an argon atmosphere to obtain ZrC aerogel. After characterization, the density of the obtained aerogel was 0.321g / cm 3 , the room temperature thermal conductivity is 0.0851 W·m -1 ·K -1 Only tetragonal zirconium dioxide (t-ZrO2) was detected in the XRD test.

[0040] Example 6

[0041] A method for synthesizing zirconium carbide aerogel using an inorganic zirconium salt and a phenolic resin comprises the following steps:

[0042] Dissolve zirconium oxychloride octahydrate in a mixed solution of ethanol and deionized water, stir for 30 minutes, then add acetic acid and N,N-dimethylformamide in turn and stir for 30 minutes to obtain ZrO2 sol. The molar ratio of zirconium oxychloride octahydrate, acetic acid and N,N-dimethylformamide is 1:1:0.5; dissolve linear phenolic resin in ethanol solution, the concentration of phenolic resin is 5wt%, add hexamethylenetetramine, stir until completely dissolved, and obtain phenolic resin sol. The amount of hexamethylenetetramine added is 5% of the mass of phenolic resin; add phenolic sol to ZrO2 sol, stir for a period of time to obtain transparent sol, wherein the mass ratio of phenolic sol to ZrO2 sol is 2:1, and place the above two-component sol in a 100℃ oven for aging for 24 hours to obtain phenolic / ZrO2 double network gel. Then, it was placed in a 60-150°C forced air drying oven for gradient drying or supercritical drying to obtain phenolic / ZrO2 double network aerogel. Finally, the phenolic / ZrO2 double network aerogel was placed in a vacuum carbonization furnace and calcined at 1400°C in an argon atmosphere to obtain ZrC aerogel. After characterization, the density of the obtained aerogel was 0.294g / cm 3, the room temperature thermal conductivity is 0.0621 W·m -1 ·K -1 The ZrC crystal phase can be detected in XRD, while the tetragonal zirconium dioxide (t-ZrO2) still exists, with a compressive strength of 2.78MPa.

[0043] The specific description above further illustrates the purpose, technical solutions and beneficial effects of the invention in detail. It should be understood that the above is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing ZrC aerogel using zirconium inorganic salt and phenolic resin, characterized in that: The steps include: Step 1, preparing ZrO2 sol: preparing an alcohol-water solution, dissolving an inorganic zirconium salt in a mixed solution of ethanol and deionized water, stirring for 30-240 minutes to fully dissolve the inorganic zirconium salt, the concentration of the inorganic zirconium salt is 0.5-2 mol / L, then adding an acid catalyst and N,N-dimethylformamide in sequence to fully hydrolyze the inorganic zirconium salt to obtain ZrO2 sol; wherein the molar ratio of the inorganic zirconium salt, the acid catalyst, and the N,N-dimethylformamide is 1:(0.5-2):(0.5-2); Step 2, preparing phenolic sol: dissolving linear phenolic resin in ethanol solution, wherein the mass fraction of linear phenolic resin is 5-50wt%, stirring until completely dissolved to obtain a transparent and uniform solution, then adding hexamethylenetetramine as a cross-linking agent, stirring until completely dissolved to obtain a phenolic resin sol; wherein the amount of the cross-linking agent added is 3-10% of the mass of the phenolic resin; Step 3, adding the phenolic sol prepared in step 2 to the ZrO2 sol in step 1, stirring for a period of time to obtain an organic-inorganic two-component sol; the mass ratio of the phenolic sol to the ZrO2 sol is 0.5-2:1; Step 4, gelation and drying: the organic-inorganic two-component sol is subjected to sol-gelation reaction in an oven at 80-100°C for 10-72h to obtain a phenolic / ZrO2 double network gel; then the sol is placed in a 60-150°C forced air drying oven for gradient temperature drying or supercritical drying to obtain a phenolic / ZrO2 double network aerogel; Step 5, carbothermal reduction: The phenolic / ZrO2 double network aerogel obtained in step 4 is subjected to high temperature carbothermal reduction reaction in an inert atmosphere or vacuum conditions to obtain ZrC aerogel.

2. The method according to claim 1, characterized in that: The inorganic zirconium salt described in step 1 is any one of zirconium oxychloride octahydrate, zirconium oxynitrate and zirconium tetrachloride.

3. The method according to claim 1, characterized in that: The acid catalyst described in step 1 is any one of acetic acid, nitric acid and hydrochloric acid.

4. The method according to claim 1, characterized in that: The temperature of high-temperature carbon thermal reduction of the phenolic / ZrO2 double network aerogel in step 5 is 800-1600°C.