A metastable lithium-rich manganese-based positive electrode material and preparation method thereof, and a lithium-ion battery
The preparation of metastable phase lithium-meng-based positive electrode material with O6-type structure through a three-step method has solved the problems of Mn migration and structural failure in the prior art, and significantly improved the cyclic performance and electrochemical performance of the material.
Patent Information
- Application Number
- CN202310346750.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-04-03
AI Technical Summary
The existing lithium-rich manganese-based positive electrode materials are prone to irreversible Mn migration during the discharge process, resulting in spinel phase generation, capacity attenuation and voltage reduction. The high-temperature sintering of traditional synthesis methods will damage the material structure and reduce cycling performance.
The three-step method is used to prepare metastable phase lithium-manganese-based positive electrode material, including high-temperature sintering to prepare sodium-containing intermediates, ion exchange preparation O2 or T2 type transition phase, and low-temperature secondary sintering to obtain O6 type structure to inhibit Mn3+/Mn4+ migrate.
Through the formation of O6-type structure, the generation of spinel phase is suppressed, and the circulation and electrochemical properties of the material are significantly improved, achieving higher first charge and discharge capacity and more stable circulation performance.
Smart Images

Figure CN116443940B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of lithium ion battery positive electrode materials, and specifically relates to a metastable lithium-rich manganese-based positive electrode material and a preparation method thereof, and a lithium ion battery. Background Art
[0002] The development of renewable energy has become an inevitable choice to replace traditional fossil energy. On the one hand, renewable energy generation using wind, light, tides, etc. is affected by the natural environment, and the power generation fluctuates greatly. Its direct connection to the grid will have an impact on the power grid, which is not conducive to the stable operation of the power grid. Therefore, the use of large-scale energy storage devices to store electricity and stably connect to the grid has become a necessary link to fully utilize renewable energy. On the other hand, with the popularization of electric vehicles, the development of batteries with higher energy density, more environmentally friendly and safer has become an urgent need. Lithium-ion batteries have great potential in both of the above fields. At present, lithium cobalt oxide and nickel cobalt manganese oxide are mainly used in the fields of electronic products and power batteries, respectively. The development of high-nickel or manganese-rich positive electrode materials has become the research focus of scientific researchers.
[0003] Lithium manganese-based materials have a higher specific capacity (>250mAh / g), and the price of manganese is lower than that of cobalt and nickel, so they are positive electrode materials with broad application prospects. At present, lithium-rich manganese-based positive electrode materials are mainly directly synthesized by a high-temperature solid-phase method. For example, Chinese patent CN102931390A discloses a preparation method of a lithium-rich manganese-based positive electrode material (xLi2MnO3-(1-x)LiMO2) (0<x<1) (M=Mn, Ni, Co, etc., one or more). The method comprises: preparing lithium salt, manganese salt and nickel salt respectively according to the general stoichiometric ratio, wet-milling and mixing, and then pre-sintering to decompose the raw salt, and wet-milling and mixing the pre-sintered product again, and then sintering to obtain a lithium-rich manganese-based positive electrode material. Chinese patent CN115676910A discloses a preparation method of a lithium-rich manganese-based positive electrode material. The lithium-rich manganese-based positive electrode material is obtained by coating a coating agent with a primary sintering product obtained from a lithium-rich manganese-based precursor and a lithium source, and the coating agent is made from a compound containing element A and a lithium source. The specific steps are: step 1, mixing the lithium-rich manganese-based precursor and the lithium source and then sintering once; step 2, mixing the compound containing element A and the lithium source to obtain a mixture; step 3, mixing the primary sintering product obtained in step 1 and the mixture obtained in step 2 and then sintering twice to obtain a lithium-rich manganese-based positive electrode material. Step 1 is to obtain the lithium-rich manganese-based positive electrode material by high-temperature sintering, and the purpose of the secondary sintering in step 3 is surface coating.
[0004] The lithium-rich manganese-based positive electrode material synthesized by the above method, whether by single sintering or multiple sintering, usually has a final sintering temperature above 800°C, so it usually has a high-temperature stable O3 type structure. However, in traditional layered manganese-based materials, manganese will be reduced to +3 valence during the discharge process, and the octahedral coordinated Mn3+ It has a strong Jahn-Teller effect. In particular, in O3-type lithium-rich manganese-based positive electrode materials, the Jahn-Teller effect will lead to irreversible migration of manganese, and finally form a spinel phase. Therefore, O3-type lithium-rich manganese-based materials usually face rapid capacity decay and voltage reduction.
[0005] Chinese patent CN114695874A discloses a method for synthesizing an O2-type lithium-rich manganese-based positive electrode material with low voltage hysteresis. The method comprises: fully grinding a sodium source and a lithium source and then calcining at high temperature to obtain a sodium-containing intermediate, and subjecting the above-mentioned sodium-containing intermediate to ion exchange in a molten lithium salt to obtain an O2-type lithium-rich manganese-based positive electrode material. The obtained material is not prone to phase transition to a spinel phase, and has a small voltage hysteresis. Although the irreversible Mn migration in the above-mentioned O2-type lithium-rich manganese-based positive electrode material can be suppressed, the ion exchange in the molten salt usually destroys the crystal structure of the material, introduces defects, reduces crystallinity, and ultimately leads to poor cycle performance.
[0006] Therefore, it is necessary to develop a structure that can inhibit irreversible Mn migration and has good crystallinity to effectively improve the cycle stability of lithium-rich manganese-based materials. Summary of the invention
[0007] The purpose of the present invention is to provide a metastable lithium-rich manganese-based positive electrode material with an O6-type structure, which can suppress the Mn 3+ / Mn 4+ The migration of the spinel phase is inhibited, thereby inhibiting the formation of the spinel phase and greatly improving the cycle performance of the material.
[0008] Another object of the present invention is to provide a method for preparing a lithium-rich manganese-based positive electrode material.
[0009] Another object of the present invention is to provide a lithium-ion battery comprising a lithium-rich manganese-based positive electrode material.
[0010] In order to achieve one of the above purposes, the present invention adopts the following technical solution:
[0011] A method for preparing a metastable lithium-rich manganese-based positive electrode material comprises the following steps:
[0012] S1, a manganese source, a lithium source, and a sodium source are sintered once to obtain a sodium-lithium-manganese-based precursor;
[0013] S2, sodium lithium manganese-based precursor and lithium salt ion exchange to obtain transition phase lithium-rich manganese-based material;
[0014] S3. The transition phase lithium-rich manganese-based material is subjected to secondary sintering at a sintering temperature of 400-600° C. to obtain a metastable phase lithium-rich manganese-based positive electrode material.
[0015] Furthermore, the molar ratio of the manganese source, lithium source and sodium source is 4:1:4, that is, the molar ratio of the three elements Mn, Li and Na is 4:1:4. If the manganese source contains nickel, the molar ratio of the three elements (Mn+Ni), Li and Na is 4:1:4.
[0016] Furthermore, the manganese source is selected from at least one of manganese carbonate, manganese hydroxide, manganese oxyhydroxide, manganese oxide, manganese trioxide, manganese dioxide, nickel manganese hydroxide, nickel manganese carbonate, and nickel manganese basic carbonate.
[0017] The molecular formula of nickel manganese hydroxide is Ni x Mn y (OH) 2(x+y) , x:y=1:(1~4);
[0018] The molecular formula of nickel manganese carbonate is Ni x Mn y (CO3) x+y , x:y=1:(1~4);
[0019] The molecular formula of nickel manganese basic carbonate is Ni x Mn y (OH) z (CO3) (x+y-z / 2) , x:y=1:(1~4).
[0020] Furthermore, the lithium source is selected from at least one of lithium carbonate, lithium hydroxide and lithium nitrate.
[0021] Furthermore, the sodium source is selected from at least one of sodium carbonate, sodium hydroxide and sodium nitrate.
[0022] Furthermore, the primary sintering temperature is 700-900° C., the sintering time is 6-24 hours, and the heating rate is 2-10° C. / min.
[0023] Furthermore, S1 is specifically as follows: mixing a manganese source, a lithium source, and a sodium source, wherein the molar ratio of the three elements of manganese, lithium, and sodium in the manganese source, lithium source, and sodium source satisfies 4:1:4, and controlling the pressure at 10 to 20 MPa for tableting, and then sintering once in an air atmosphere, the sintering temperature is controlled at 700 to 900°C, the sintering time is 6 to 24 hours, and the heating rate is 2 to 10°C / min. After cooling, taking out the sintered material and grinding it fully to obtain a powdered sample, which is a sodium-lithium-manganese-based precursor.
[0024] Furthermore, the lithium salt is selected from at least one of lithium bromide, lithium sulfate, lithium nitrate and lithium chloride, and the mass ratio of the sodium lithium manganese-based precursor to the lithium salt is 1:(8.2-11.8). The lithium salt is preferably lithium nitrate and lithium chloride, and the mass ratio of the sodium lithium manganese-based precursor, lithium nitrate and lithium chloride is 1:(6.4-8.2):(1.8-3.6).
[0025] Furthermore, S2 is specifically as follows: a sodium lithium manganese-based precursor, lithium nitrate and lithium chloride are mixed in a mass ratio of 1: (6.4-8.2): (1.8-3.6), and then heated to 260-350°C in an air atmosphere, the heating time is controlled at 2-12h, and the heating rate is 2-10°C / min; after cooling, the resulting mixture is dispersed in an aqueous solution, and filtered, washed and dried, the drying temperature is controlled at 60-150°C, and the drying time is 6-24h; after cooling, the dried sample is fully ground to obtain a powder sample, which is a transition phase lithium-rich manganese-based material.
[0026] Further, in step S2, sodium lithium manganese-based precursor powder, lithium nitrate and lithium chloride are mixed in a mass ratio of 1: (6.4-8.2): (1.8-3.6), dispersed or dissolved in an aqueous solution, stirred for 12-48 hours at a temperature range of 25-80° C., and filtered, washed and dried to obtain a powder sample.
[0027] Furthermore, the secondary sintering temperature is 450-550°C.
[0028] Furthermore, S3 is specifically as follows: pressing the transition phase lithium-rich manganese-based material into tablets, controlling the pressure at 10-20 MPa, and then performing secondary sintering in an air atmosphere, controlling the sintering temperature at 400-600°C, the sintering time at 6-24h, and the heating rate at 2-10°C / min. After cooling, taking out the secondary sintered material and grinding it thoroughly to obtain a powdered sample, which is a metastable phase lithium-rich manganese-based positive electrode material.
[0029] During the secondary sintering process, the lithium-rich manganese-based material will change from the O2 transition phase to the O6 metastable phase. Although the prior art also uses secondary sintering, the first sintering is low-temperature pre-sintering or ion exchange to obtain oxide precursors and other structures, and no lithium-rich manganese-based material is obtained. The secondary sintering to form the lithium-rich manganese-based material is still high-temperature sintering, and the O3 structure is obtained.
[0030] A metastable lithium-rich manganese-based positive electrode material is prepared by the above-mentioned preparation method.
[0031] A positive electrode sheet comprises the above-mentioned metastable lithium-rich manganese-based positive electrode material.
[0032] A lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator, an electrolyte and a shell, and contains the above-mentioned metastable phase lithium-rich manganese-based positive electrode material.
[0033] The present invention has the following beneficial effects:
[0034] Traditional lithium-rich manganese-based materials are prepared by high-temperature solid-phase method, and the final sintering temperature is above 800℃, so the obtained material is in a high-temperature stable O3 type structure. As the cycle proceeds, Mn 3+ / Mn 4+ The irreversible migration of Mn is getting more serious, leading to the formation of spinel phase, capacity and voltage decay. Lithium-rich manganese-based materials that undergo ion exchange in molten lithium salts through sodium-containing intermediates usually have an O2-type structure, in which irreversible Mn migration can be suppressed, but ion exchange in molten salts usually destroys the crystal structure of the material, introduces defects, and reduces crystallinity.
[0035] The present invention adopts a three-step method, including high-temperature sintering to prepare a sodium-containing intermediate, ion exchange to prepare a transition phase with an O2 or T2 type structure, and low-temperature sintering to obtain a metastable lithium-rich manganese-based positive electrode material with an O6 type structure.
[0036] The O6 type structure has not been reported in the prior art and is synthesized for the first time by the present invention. It is unstable at high temperatures and will decompose into an O3 type structure and release oxygen. Therefore, the sintering temperature is the key and its synthesis must be strictly controlled at a temperature of 400-600°C.
[0037] The crystal structure of the O6 metastable phase is different from that of the O3 stable phase obtained by traditional high-temperature sintering. In the traditional stable phase, the Li and Mn layers are stacked in a coplanar manner, and transition metal migration is easy to occur. The O6-type metastable lithium-rich manganese-based material has a stable coplanar local structure. The Li and Mn layers are stacked in a coplanar manner. The transition metal migration is repelled by the Li layer and is not easy to occur, which can inhibit the Mn 3+ / Mn 4+ The irreversible migration of the spinel phase is inhibited, thereby inhibiting the formation of the spinel phase and greatly improving the cycle performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a scanning electron microscope image of a metastable lithium-rich manganese-based material having an O6-type structure in Example 1;
[0039] Figure 2 This is the XRD pattern of the metastable lithium-rich manganese-based material with O6-type structure in Example 1;
[0040] Figure 3 This is the XRD pattern of the lithium-rich manganese-based material with O3-type structure in Comparative Example 1;
[0041] Figure 4This is the XRD pattern of the lithium-rich manganese-based material with O2-type structure in Comparative Example 2;
[0042] Figure 5 The charge and discharge curve of the lithium battery containing the positive electrode material of Example 1;
[0043] Figure 6 The charge and discharge curve of the lithium battery containing the positive electrode material of Comparative Example 1;
[0044] Figure 7 The charge and discharge curve of the lithium battery containing the positive electrode material of Comparative Example 2;
[0045] Figure 8 This is a scanning electron microscope image of a metastable lithium-rich nickel-manganese-based material having an O6-type structure in Example 2;
[0046] Fig. 9 This is the XRD pattern of the metastable lithium-rich nickel-manganese-based material with O6-type structure in Example 2;
[0047] Fig.10 This is the XRD pattern of the lithium-rich nickel-manganese-based material with O3-type structure in Comparative Example 3;
[0048] Fig.11 This is the XRD pattern of the lithium-rich nickel-manganese-based material with O2+T2 structure of Comparative Example 4;
[0049] Fig.12 The charge and discharge curve of the lithium battery containing the positive electrode material of Example 2;
[0050] Fig.13 The charge and discharge curve of the lithium battery containing the positive electrode material of Comparative Example 3;
[0051] Fig.14 The charge and discharge curve of the lithium battery containing the positive electrode material of Comparative Example 4;
[0052] Fig.15 This is a cycle performance diagram of a lithium battery containing the positive electrode material of Example 2;
[0053] Fig.16 This is a cycle performance diagram of a lithium battery containing the positive electrode material of Comparative Example 3. DETAILED DESCRIPTION
[0054] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0055] Example 1
[0056] This embodiment provides a metastable lithium-rich manganese-based positive electrode material with a chemical formula of Li 1+x Mn 0.8 O2 (0≤x≤0.2), the preparation method steps are as follows:
[0057] S1. Mix manganese carbonate, lithium carbonate and sodium carbonate in a molar ratio of 8:1:4, and press the tablets under the pressure of 15 MPa, and then sinter them once in an air atmosphere. The sintering temperature is controlled at 800°C, the sintering time is 12 hours, and the heating rate is 5°C / min. After cooling, take out the sintered material and grind it thoroughly to obtain a powder sample, which is a sodium-lithium-manganese-based precursor;
[0058] S2. Sodium lithium manganese-based precursor powder, lithium nitrate and lithium chloride are mixed in a mass ratio of 1:8.2:1.8, and then heated to 280°C in an air atmosphere, the heating time is controlled at 4h, and the heating rate is 5°C / min; after cooling, the obtained mixture is dispersed in an aqueous solution, stirred for 28h at a temperature range of 50°C, and filtered, washed and dried, the drying temperature is controlled at 120°C, and the drying time is 12h; after cooling, the dried sample is fully ground to obtain a powder sample, which is a transition phase lithium-rich manganese-based material;
[0059] S3, the transition phase lithium-rich manganese-based material is pressed into tablets, the pressure is controlled at 15Mpa, and then secondary sintering is performed in an air atmosphere, the sintering temperature is controlled at 500℃, the sintering time is 12h, and the heating rate is 2℃ / min. After cooling, the secondary sintered material is taken out and fully ground to obtain a powder sample, which is the metastable phase lithium-rich manganese-based positive electrode material. The scanning electron microscope image is as follows Figure 1 As shown in the figure (the text in the electron microscope image in this article has no other meaning except for necessary information such as magnification and length), the secondary particle size of the positive electrode material is several tens of microns, in which the secondary particles are accumulated by primary particles of 2 to 5 microns, with a smooth surface and no impurities. Figure 2 As shown, it has an O6-type metastable phase structure, sharp diffraction peaks, high intensity, no impurities, and intact crystal form.
[0060] Comparative Example 1
[0061] In this comparative example, the conventional high temperature solid phase method was used to prepare the O3 phase lithium-rich manganese-based positive electrode material, whose chemical formula is Li 1.2 Mn 0.8 O2. The specific steps are:
[0062] Manganese carbonate and lithium carbonate were mixed in a molar ratio of 4:3, and the pressure was controlled at 15Mpa for tableting, and then sintered in an air atmosphere, the sintering temperature was controlled at 800℃, the sintering time was 12h, and the heating rate was 5℃ / min. After cooling, the sintered material was taken out and fully ground to obtain a powdered sample, which is the O3 phase lithium-rich manganese-based positive electrode material. Its XRD pattern is as follows Figure 3 As shown, it has a stable phase structure of O3 type, sharp diffraction peaks, high intensity, no impurities, and intact crystal form.
[0063] Comparative Example 2
[0064] In this comparative example, a sodium-containing intermediate was prepared by a high-temperature solid phase method, and a lithium-rich manganese-based positive electrode material with an O2-type structure was prepared by ion exchange, and its chemical formula is Li 1+x Mn 0.8 O2(0≤x≤0.2). The specific steps are:
[0065] S1. Mix manganese carbonate, lithium carbonate and sodium carbonate in a molar ratio of 8:1:4, and press the tablets under the pressure of 15 MPa, and then sinter them once in an air atmosphere. The sintering temperature is controlled at 800°C, the sintering time is 12 hours, and the heating rate is 5°C / min. After cooling, take out the sintered material and grind it thoroughly to obtain a powder sample, which is a sodium-lithium-manganese-based precursor;
[0066] S2. Mix sodium lithium manganese-based precursor powder, lithium nitrate and lithium chloride in a mass ratio of 1:8.2:1.8, and then heat to 280°C in an air atmosphere, with the heating time controlled at 4h and the heating rate at 5°C / min; after cooling, disperse the resulting mixture in an aqueous solution, stir for 28h at a temperature range of 50°C, and filter, wash and dry, with the drying temperature controlled at 120°C and the drying time at 12h; after cooling, fully grind the dried sample to obtain a powder sample, which is a lithium-rich manganese-based material with an O2 structure. Its XRD pattern is as follows Figure 4 As shown, the positive electrode material has an O2 type structure, sharp diffraction peaks, high intensity, no impurities, intact crystal form, and presents a preferred orientation of the (002) crystal plane.
[0067] Performance Testing
[0068] The metastable lithium-rich manganese-based positive electrode material with an O6-type structure in Example 1, the O3-type lithium-rich manganese-based positive electrode material in Comparative Example 2, and the O2-type lithium-rich manganese-based positive electrode material in Comparative Example 3 were used as active materials to make button batteries, respectively, and the performance tests were carried out. The specific production methods and test conditions are as follows:
[0069] The positive electrode material is mixed with conductive carbon black and binder PVDF in a mass ratio of 8:1:1, and a slurry is prepared with N-methylpyrrolidone as a solvent, coated on an aluminum foil current collector, and vacuum dried at 120°C for 12 hours to obtain a positive electrode sheet. The positive electrode sheet is cut into a disc with a diameter of 12 mm and assembled with a metal lithium sheet and a polypropylene separator into a CR2016 type battery. The electrolyte is a solvent of ethylene carbonate and dimethyl carbonate mixed in a volume ratio of 1:1, and LiPF6 is the electrolyte salt with a concentration of 1 mol / L. The battery assembly process should be completed in an argon-protected glove box.
[0070] The battery is tested for charge and discharge performance. The results are as follows Figures 5 to 7 As shown, the first discharge capacity of the O6 type metastable phase lithium-rich manganese-based positive electrode material reaches 308 mAh / g, which is much larger than the 12 mAh / g of the O3 type lithium-rich manganese-based positive electrode material, and larger than the 233 mAh / g of the O2 type lithium-rich manganese-based positive electrode material. The O6 type metastable phase lithium-rich manganese-based positive electrode material of the present invention has a higher first charge and discharge capacity.
[0071] Example 2
[0072] This embodiment provides a metastable lithium-rich nickel-manganese-based positive electrode material with a chemical formula of Li 1+x Ni 0.2 Mn 0.6 O2 (0≤x≤0.2), the preparation method steps are as follows:
[0073] S1. Mix binary nickel manganese carbonate NiMn3(CO3)4, lithium carbonate and sodium carbonate in a molar ratio of 2:1:4, and control the pressure at 15 MPa for tableting, and then sinter once in an air atmosphere, the sintering temperature is controlled at 800°C, the sintering time is 12h, and the heating rate is 5°C / min. After cooling, take out the sintered material and grind it fully to obtain a powder sample, which is a sodium-lithium-nickel-manganese-based precursor;
[0074] S2. Sodium lithium manganese-based precursor powder, lithium nitrate and lithium chloride are mixed in a mass ratio of 1:8.2:1.8, and then heated to 280°C in an air atmosphere, the heating time is controlled at 4h, and the heating rate is 5°C / min; after cooling, the obtained mixture is dispersed in an aqueous solution, stirred for 28h at a temperature range of 50°C, and filtered, washed and dried, the drying temperature is controlled at 120°C, and the drying time is 12h; after cooling, the dried sample is fully ground to obtain a powder sample, which is a transition phase lithium-rich nickel-manganese-based material;
[0075] S3, the transition phase lithium-rich nickel-manganese-based material is pressed into tablets, the pressure is controlled at 15Mpa, and then secondary sintering is performed in an air atmosphere, the sintering temperature is controlled at 550℃, the sintering time is 12h, and the heating rate is 2℃ / min. After cooling, the secondary sintered material is taken out and fully ground to obtain a powder sample, which is a metastable lithium-rich nickel-manganese-based positive electrode material. The scanning electron microscope image is as follows Figure 8 As shown in the figure, the secondary particles of the positive electrode material are spherical with a size of 10 to 20 microns, and the secondary particles are formed by the accumulation of primary particles with a size of several hundred nanometers. The primary particles are flat and have a smooth surface without impurities. Fig. 9 As shown, it has an O6-type metastable phase structure, sharp diffraction peaks, high intensity, no impurities, and intact crystal form.
[0076] Comparative Example 3
[0077] In this comparative example, the conventional high temperature solid phase method was used to prepare the O3 phase lithium-rich nickel-manganese-based positive electrode material, whose chemical formula is Li 1.2 Ni 0.2 Mn 0.6 O2. The specific steps are:
[0078] Spherical binary nickel manganese carbonate NiMn3(CO3)4 and lithium carbonate are mixed in a molar ratio of 1:3, and the pressure is controlled at 15Mpa for tableting, and then sintered in an air atmosphere, the sintering temperature is controlled at 800℃, the sintering time is 12h, and the heating rate is 5℃ / min. After cooling, the sintered material is taken out and fully ground to obtain a powder sample, which is the O3 phase lithium-rich nickel manganese-based positive electrode material. Its XRD pattern is as follows Fig.10 As shown, it has a stable phase structure of O3 type, sharp diffraction peaks, high intensity, no impurities, and intact crystal form.
[0079] Comparative Example 4
[0080] In this comparative example, a sodium-containing intermediate was prepared by a high-temperature solid phase method, and a lithium-rich nickel-manganese-based positive electrode material with an O2+T2 structure was prepared by ion exchange, and its chemical formula is Li 1+x Ni 0.2 Mn 0.6 O2(0≤x≤0.2). The specific steps are:
[0081] S1. Mix binary nickel manganese carbonate NiMn3(CO3)4, lithium carbonate and sodium carbonate in a molar ratio of 2:1:4, and control the pressure at 15 MPa for tableting, and then sinter once in an air atmosphere, the sintering temperature is controlled at 800°C, the sintering time is 12h, and the heating rate is 5°C / min. After cooling, take out the sintered material and grind it fully to obtain a powder sample, which is a sodium-lithium-nickel-manganese-based precursor;
[0082] S2. Mix sodium lithium manganese-based precursor powder, lithium nitrate and lithium chloride in a mass ratio of 1:8.2:1.8, and then heat to 280°C in an air atmosphere, with the heating time controlled at 4h and the heating rate at 5°C / min; after cooling, disperse the resulting mixture in an aqueous solution, stir for 28h at a temperature range of 50°C, and filter, wash and dry, with the drying temperature controlled at 120°C and the drying time at 12h; after cooling, fully grind the dried sample to obtain a powder sample, which is a transition phase lithium-rich nickel-manganese-based material. Its XRD pattern is as follows Fig.11 As shown, the positive electrode material has an O2-type and T2-type composite structure, sharp diffraction peaks, high intensity, no impurities, intact crystal form, and presents a preferred orientation of the (002) crystal plane.
[0083] Performance Testing
[0084] The metastable lithium-rich nickel-manganese-based positive electrode material with an O6-type structure in Example 2, the O3-type lithium-rich nickel-manganese-based positive electrode material in Comparative Example 3, and the O2+T2-type lithium-rich nickel-manganese-based positive electrode material in Comparative Example 4 were used as active materials to make button batteries, respectively, and the performance tests were carried out. The specific production methods and test conditions are as follows:
[0085] The positive electrode material is mixed with conductive carbon black and binder PVDF in a mass ratio of 8:1:1, and a slurry is prepared with N-methylpyrrolidone as a solvent, coated on an aluminum foil current collector, and vacuum dried at 120°C for 12 hours to obtain a positive electrode sheet. The positive electrode sheet is cut into a disc with a diameter of 12 mm and assembled with a metal lithium sheet and a polypropylene separator into a CR2016 type battery. The electrolyte is a solvent of ethylene carbonate and dimethyl carbonate mixed in a volume ratio of 1:1, and LiPF6 is the electrolyte salt with a concentration of 1 mol / L. The battery assembly process should be completed in an argon-protected glove box.
[0086] The battery is tested for charge and discharge performance. The results are as follows Figures 12-14 As shown in the figure, the electrochemical behavior of O6-type metastable lithium-rich nickel-manganese-based cathode materials is completely different from that of traditional O3-type lithium-rich nickel-manganese-based cathode materials and O2+T2-type lithium-rich nickel-manganese-based cathode materials. It has a highly reversible phase change process in the high voltage range (4.5-4.8V), while in O3 or O2+T2-type materials, there is no capacity in the high voltage range. This is because O3-type materials usually undergo an O3-O1 phase change process in the high voltage range, which leads to Mn migration and causes surface densification and irreversible structural damage of the material; O6-type metastable phase materials undergo a highly reversible O6-O2 phase change, and the coplanar local structure is maintained, so that Mn migration is effectively suppressed.
[0087] The cycling performance of O6-type metastable lithium-rich nickel-manganese-based cathode material and traditional O3-type lithium-rich nickel-manganese-based cathode material was tested. Figures 15-16 As shown in the figure, at a current density of 100mA / g, the initial specific capacity of the O3-type lithium-rich nickel-manganese-based cathode material is 121.1mAh / g, which reaches 137mAh / g after 40 cycles, and finally drops to 128.9mAh / g after 100 cycles. The initial specific capacity of the O6-type metastable lithium-rich nickel-manganese-based cathode material is 256.9mAh / g, and the capacity is still 194.2mAh / g after 100 cycles, which is much higher than the highest specific capacity of the O3-type lithium-rich nickel-manganese-based cathode material.
[0088] Example 3
[0089] This embodiment provides a metastable lithium-rich manganese-based positive electrode material with a chemical formula of Li 1+x Mn 0.8 O2 (0≤x≤0.2), the preparation method steps are as follows:
[0090] S1. Manganese dioxide, lithium carbonate and sodium carbonate are mixed in a molar ratio of 8:1:4, and the pressure is controlled at 15 MPa for tableting, followed by sintering once in an air atmosphere, the sintering temperature is controlled at 800°C, the sintering time is 12 hours, and the heating rate is 5°C / min. After cooling, the sintered material is taken out and fully ground to obtain a powder sample, which is a sodium-lithium-manganese-based precursor;
[0091] S2. Sodium lithium manganese-based precursor powder, lithium nitrate and lithium chloride are mixed in a mass ratio of 1:8.2:1.8, and then heated to 280°C in an air atmosphere, the heating time is controlled at 4h, and the heating rate is 5°C / min; after cooling, the obtained mixture is dispersed in an aqueous solution, stirred for 28h at a temperature range of 50°C, and filtered, washed and dried, the drying temperature is controlled at 120°C, and the drying time is 12h; after cooling, the dried sample is fully ground to obtain a powder sample, which is a transition phase lithium-rich manganese-based material;
[0092] S3. Press the transition phase lithium-rich manganese-based material into tablets, control the pressure at 15 MPa, and then perform secondary sintering in an air atmosphere. The sintering temperature is controlled at 450°C, the sintering time is 12 hours, and the heating rate is 2°C / min. After cooling, take out the secondary sintered material and grind it thoroughly to obtain a powder sample, which is a metastable phase lithium-rich manganese-based positive electrode material.
[0093] Example 4
[0094] This embodiment provides a metastable lithium-rich manganese-based positive electrode material, and the preparation method steps are as follows:
[0095] S1. Manganese hydroxide, lithium carbonate and sodium carbonate are mixed in a molar ratio of 8:1:4, and the pressure is controlled at 12 MPa for tableting, followed by sintering once in an air atmosphere, the sintering temperature is controlled at 900°C, the sintering time is 8 hours, and the heating rate is 8°C / min. After cooling, the sintered material is taken out and fully ground to obtain a powdered sample, which is a sodium-lithium-manganese-based precursor;
[0096] S2. Sodium lithium manganese-based precursor powder, lithium nitrate and lithium chloride are mixed in a mass ratio of 1:6.4:3.6, and then heated to 300°C in an air atmosphere, the heating time is controlled at 8h, and the heating rate is 6°C / min; after cooling, the obtained mixture is dispersed in an aqueous solution, stirred for 36h at a temperature range of 40°C, and filtered, washed and dried, the drying temperature is controlled at 140°C, and the drying time is 22h; after cooling, the dried sample is fully ground to obtain a powder sample, which is a transition phase lithium-rich manganese-based material;
[0097] S3. Press the transition phase lithium-rich manganese-based material into tablets, control the pressure at 10 MPa, and then perform secondary sintering in an air atmosphere. The sintering temperature is controlled at 500°C, the sintering time is 8 hours, and the heating rate is 8°C / min. After cooling, take out the secondary sintered material and grind it thoroughly to obtain a powdered sample, which is a metastable phase lithium-rich manganese-based positive electrode material.
[0098] Example 5
[0099] This embodiment provides a metastable lithium-rich manganese-based positive electrode material, and the preparation method steps are as follows:
[0100] S1. Manganese oxide, lithium hydroxide and sodium hydroxide are mixed in a molar ratio of 4:1:4, and the pressure is controlled at 20 MPa for tableting, followed by sintering once in an air atmosphere, the sintering temperature is controlled at 700°C, the sintering time is 20 hours, and the heating rate is 10°C / min. After cooling, the sintered material is taken out and fully ground to obtain a powdered sample, which is a sodium-lithium-manganese-based precursor;
[0101] S2. Sodium lithium manganese-based precursor powder, lithium nitrate and lithium chloride are mixed in a mass ratio of 1:7.0:2.5, and then heated to 330°C in an air atmosphere, the heating time is controlled at 10 hours, and the heating rate is 4°C / min; after cooling, the obtained mixture is dispersed in an aqueous solution, stirred at a temperature range of 70°C for 48 hours, and filtered, washed and dried, the drying temperature is controlled at 100°C, and the drying time is 6 hours; after cooling, the dried sample is fully ground to obtain a powder sample, which is a transition phase lithium-rich manganese-based material;
[0102] S3. Press the transition phase lithium-rich manganese-based material into tablets, control the pressure at 14 MPa, and then perform secondary sintering in an air atmosphere. The sintering temperature is controlled at 400°C, the sintering time is 15 hours, and the heating rate is 6°C / min. After cooling, take out the secondary sintered material and grind it thoroughly to obtain a powdered sample, which is a metastable phase lithium-rich manganese-based positive electrode material.
[0103] Example 6
[0104] This embodiment provides a metastable lithium-rich manganese-based positive electrode material, and the preparation method steps are as follows:
[0105] S1. Nickel manganese hydroxide NiMn(OH)4, lithium nitrate and sodium nitrate are mixed in a molar ratio of 2:1:4, and the pressure is controlled at 17 MPa for tableting, followed by sintering once in an air atmosphere, the sintering temperature is controlled at 750°C, the sintering time is 16 hours, and the heating rate is 2°C / min. After cooling, the sintered material is taken out and fully ground to obtain a powdered sample, which is a sodium-lithium-manganese-based precursor;
[0106] S2. Sodium lithium manganese-based precursor powder, lithium nitrate and lithium chloride are mixed in a mass ratio of 1:7.6:3.0, and then heated to 350°C in an air atmosphere, the heating time is controlled at 6h, and the heating rate is 10°C / min; after cooling, the obtained mixture is dispersed in an aqueous solution, stirred at a temperature range of 60°C for 24h, and filtered, washed and dried, the drying temperature is controlled at 80°C, and the drying time is 15h; after cooling, the dried sample is fully ground to obtain a powder sample, which is a transition phase lithium-rich manganese-based material;
[0107] S3. Press the transition phase lithium-rich manganese-based material into tablets, control the pressure at 18 MPa, and then perform secondary sintering in an air atmosphere. The sintering temperature is controlled at 600°C, the sintering time is 20 hours, and the heating rate is 4°C / min. After cooling, take out the secondary sintered material and grind it thoroughly to obtain a powder sample, which is a metastable phase lithium-rich manganese-based positive electrode material.
[0108] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing a metastable lithium-rich manganese-based positive electrode material, characterized in that: The following steps are involved: S1, a manganese source, a lithium source, and a sodium source are sintered once to obtain a sodium-lithium-manganese-based precursor; S2, sodium lithium manganese-based precursor and lithium salt ion exchange to obtain transition phase lithium-rich manganese-based material; S3, the transition phase lithium-rich manganese-based material is subjected to secondary sintering at a sintering temperature of 400-600° C. to obtain a metastable phase lithium-rich manganese-based positive electrode material; After the secondary sintering, the lithium-rich manganese-based material changes from an O2-type or T2-type transition phase to an O6-type metastable phase; The chemical formula of the metastable lithium-rich manganese-based positive electrode material is Li 1+x Mn 0.8 O2, where 0≤x≤0.2, or Li 1+ x Ni 0.2 Mn 0.6 O2, where 0≤x≤0.2; The molar ratio of manganese, lithium and sodium in the manganese source, lithium source and sodium source is 4:1:4; the primary sintering temperature is 700-900°C, the sintering time is 6-24h, and the heating rate is 2-10°C / min; The S2 is specifically as follows: a sodium lithium manganese-based precursor, lithium nitrate and lithium chloride are mixed in a mass ratio of 1: (6.4-8.2): (1.8-3.6), and then heated to 260-350° C. in an air atmosphere, the heating time is controlled at 2-12 hours, and the heating rate is 2-10° C. / min; after cooling, the obtained mixture is dispersed in an aqueous solution, and filtered, washed and dried, the drying temperature is controlled at 60-150° C., and the drying time is 6-24 hours; after cooling, the dried sample is ground to obtain a transition phase lithium-rich manganese-based material; The S3 is specifically as follows: pressing the transition phase lithium-rich manganese-based material into tablets, controlling the pressure at 10-20 MPa, and then performing secondary sintering in an air atmosphere, controlling the sintering temperature at 400-600°C, the sintering time at 6-24h, and the heating rate at 2-10°C / min. After cooling, taking out the secondary sintered material and grinding it to obtain a metastable lithium-rich manganese-based positive electrode material.
2. The preparation method according to claim 1, characterized in that: The manganese source is selected from at least one of manganese carbonate, manganese hydroxide, manganese oxyhydroxide, manganese oxide, manganese trioxide, manganese dioxide, nickel manganese hydroxide, nickel manganese carbonate, and nickel manganese basic carbonate; the lithium source is selected from at least one of lithium carbonate, lithium hydroxide, and lithium nitrate; and the sodium source is selected from at least one of sodium carbonate, sodium hydroxide, and sodium nitrate.
3. The preparation method according to claim 1, characterized in that: The S1 is specifically as follows: a manganese source, a lithium source and a sodium source are mixed, wherein the molar ratio of the three elements of manganese, lithium and sodium in the manganese source, the lithium source and the sodium source satisfies 4:1:4, and the pressure is controlled at 10-20 MPa for tableting, followed by sintering once in an air atmosphere, the sintering temperature is controlled at 700-900°C, the sintering time is 6-24h, the heating rate is 2-10°C / min, and after cooling, the sintered material is taken out and ground to obtain a sodium-lithium-manganese-based precursor.
4. The preparation method according to claim 1, characterized in that: The lithium salt is selected from at least one of lithium bromide, lithium sulfate, lithium nitrate and lithium chloride, and the mass ratio of the sodium lithium manganese-based precursor to the lithium salt is 1:(8.2-11.8).
5. A metastable lithium-rich manganese-based positive electrode material, characterized in that: The metastable lithium-rich manganese-based positive electrode material is prepared by the preparation method according to any one of claims 1 to 4.
6. A positive electrode sheet, characterized in that: The positive electrode sheet comprises the metastable lithium-rich manganese-based positive electrode material as described in claim 5.
7. A lithium ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator, an electrolyte and a casing, characterized in that: The positive electrode sheet is as described in claim 6.