Chiral liquid crystal polymer and preparation method thereof

By introducing amylose into the liquid crystal polymer structure, a chiral liquid crystal polymer is prepared, which solves the problem of insufficient optical performance of existing liquid crystal polymers and achieves excellent performance in the field of photoelectricity.

CN116444775BActive Publication Date: 2024-11-05NINGXIA QINGYAN POLYMER MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310108156.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-13
Publication Date
2024-11-05
Estimated Expiration
2043-02-13

AI Technical Summary

Technical Problem

The existing liquid crystal polymers have insufficient optical properties in the field of photoelectricity, making it difficult to meet the needs of high-quality chiral liquid crystal polymers.

Method used

By introducing amylose as chiral units into the liquid crystal polymer structure, using its rich hydroxyl groups for modification, chiral liquid crystal polymer was prepared, and after reflux reaction was performed using amylose acetate, parahydroxybiphenol and azelayl chloride. Acidification was performed to obtain a chiral liquid crystal polymer.

Benefits of technology

The chiral properties of liquid crystal polymers have been realized, their optical properties have been improved, and their economic and application value have been achieved in the field of optoelectronics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116444775B_ABST
    Figure CN116444775B_ABST
Patent Text Reader

Abstract

The present application relates to a chiral liquid crystal polymer and a preparation method thereof, and belongs to the technical field of polymer materials; the method comprises: obtaining amylose acetate; dissolving the amylose acetate, p-hydroxydiphenol and azelaic acid chloride in a solvent to obtain a mixture; subjecting the mixture to a reflux reaction, and then acidifying to obtain a chiral liquid crystal polymer; utilizing the characteristics of amylose having abundant hydroxyl groups on its surface and being easy to modify, by introducing the side chains of the liquid crystal polymer into the amylose, the liquid crystal polymer is endowed with chiral properties, thereby having excellent optical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer materials, and in particular to a chiral liquid crystal polymer and a preparation method thereof. Background Art

[0002] Liquid crystal polymers include side chain liquid crystal polymers and main chain liquid crystal polymers. Side chain liquid crystal polymers are different from main chain liquid crystal polymers. The main chain only serves to connect liquid crystal units. Their properties are mainly determined by the mesogens at the side chain positions and are little affected by the polymer main chain. Therefore, by introducing different side chains, liquid crystal polymers can have different properties. For example, by introducing flexible side chains, the properties of the polymer can have chain flexibility. Side chains include polysiloxanes, poly (meth) acrylates, polyethers and polyvinyl alcohols, among which (meth) acrylates have better flexibility.

[0003] In recent years, material science has developed rapidly, especially liquid crystal polymers. It has been found that chiral liquid crystal polymers have many excellent properties, especially the optical properties of chiral polymers. Their excellent optical properties can be used in the optoelectronic field. Therefore, the development of high-quality chiral liquid crystal polymers has important economic and application value. Summary of the invention

[0004] The present application provides a chiral liquid crystal polymer and a preparation method thereof, so as to provide a new chiral liquid crystal polymer.

[0005] In a first aspect, the present application provides a method for preparing a chiral liquid crystal polymer, the method comprising:

[0006] Obtaining amylose acetate;

[0007] dissolving the amylose acetate, p-hydroxydiphenol and azelaic acid chloride in a solvent to obtain a mixture;

[0008] The mixture is subjected to a reflux reaction and then acidified to obtain a chiral liquid crystal polymer.

[0009] As an optional embodiment, the step of obtaining amylose acetate specifically comprises:

[0010] Dissolve the amylose and hydroxyl protective agent in a solvent, then perform a first reaction and concentrate to obtain a viscous liquid;

[0011] The viscous liquid and acetic anhydride are mixed, and then a second reaction is performed to obtain an intermediate;

[0012] The intermediate is mixed with acetic acid, and then subjected to a third reaction to obtain amylose acetate.

[0013] As an optional embodiment, the hydroxyl protecting agent includes at least one of DMT and tert-butyldimethylsilyl chloride.

[0014] As an optional embodiment, the temperature of the first reaction is 5-15°C; and / or

[0015] The first reaction time is 4-6 hours.

[0016] As an optional embodiment, the temperature of the second reaction is 90-95°C; and / or

[0017] The second reaction time is 4-6 hours.

[0018] As an optional embodiment, the temperature of the third reaction is 30-40° C.; and / or

[0019] The time of the third reaction is 4-6h.

[0020] As an optional embodiment, in the mixture, the mass proportion of the amylose acetate is 1%-30%.

[0021] As an optional implementation, the acidified acidic solution includes hydrochloric acid, and the volume concentration of the hydrochloric acid is 40%-60%.

[0022] In a second aspect, the present application provides a chiral liquid crystal polymer, which is prepared by the preparation method of the chiral liquid crystal polymer provided in the first aspect.

[0023] As an optional embodiment, the chiral liquid crystal polymer has the structural formula:

[0024]

[0025] Wherein, m and n are independently selected from positive integers.

[0026] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0027] The method provided in the embodiment of the present application can prepare a new chiral liquid crystal polymer, which utilizes the fact that the surface of amylose has abundant hydroxyl groups and is easy to modify. By introducing the side chains of the liquid crystal polymer into the amylose, the liquid crystal polymer has chiral properties and thus has excellent optical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0029] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0030] Figure 1 A flowchart of a method provided in an embodiment of the present application. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0032] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0033] Liquid crystal polymers include side chain liquid crystal polymers and main chain liquid crystal polymers. Side chain liquid crystal polymers are different from main chain liquid crystal polymers. The main chain only serves to connect liquid crystal units. Their properties are mainly determined by the mesogens at the side chain positions and are little affected by the polymer main chain. Therefore, by introducing different side chains, liquid crystal polymers can have different properties. For example, by introducing flexible side chains, the properties of the polymer can have chain flexibility. Side chains include polysiloxanes, poly (meth) acrylates, polyethers and polyvinyl alcohols, among which (meth) acrylates have better flexibility.

[0034] In recent years, material science has developed rapidly, especially liquid crystal polymers. It has been found that chiral liquid crystal polymers have many excellent properties, especially the optical properties of chiral polymers. Their excellent optical properties can be used in the optoelectronic field. Therefore, the development of high-quality chiral liquid crystal polymers has important economic and application value.

[0035] The applicant discovered that amylose has a chiral structure and has abundant hydroxyl groups on its surface, which makes it easy to modify. Therefore, the applicant intends to introduce amylose as a chiral unit into the liquid crystal polymer structural unit to make the liquid crystal polymer have chiral properties, thereby having excellent optical properties.

[0036] like Figure 1 As shown, the present application embodiment provides a method for preparing a chiral liquid crystal polymer, the method comprising:

[0037] S1. Obtaining amylose acetate;

[0038] In some embodiments, obtaining amylose acetate specifically comprises:

[0039] S1.1. Dissolve amylose and hydroxyl protective agent in a solvent, then perform a first reaction and concentrate to obtain a viscous liquid; the structural formula of amylose is:

[0040]

[0041] Wherein, n is any positive integer.

[0042] In some embodiments, the hydroxyl protecting agent includes at least one of DMT and tert-butyldimethylsilyl chloride, preferably tert-butyldimethylsilyl chloride. The temperature of the first reaction is 5-15° C., preferably 10° C.; the time of the first reaction is 4-6 hours, preferably 5 hours.

[0043] Specifically, in this embodiment, 20 g of amylose, 20 g of tert-butyldimethylsilyl chloride and 100 ml of pyridine were added to a reaction bottle, and the reaction was carried out at 10 degrees Celsius for 5 hours. After the reaction was completed, the crude product was evaporated under reduced pressure to obtain a viscous liquid.

[0044] S1.2. The viscous liquid and acetic anhydride are mixed, and then a second reaction is performed to obtain an intermediate;

[0045] In some embodiments, the temperature of the second reaction is 90-95°C, preferably 95°C, and the time of the second reaction is 4-6h, preferably 5h.

[0046] Specifically, in this embodiment, 100 ml of acetic anhydride was added to the viscous liquid, and the reaction was carried out at 95 degrees Celsius for 5 hours to obtain an intermediate.

[0047] S1.3. The intermediate and acetic acid are mixed, and then a third reaction is performed to obtain amylose acetate. The structural formula of amylose acetate is:

[0048]

[0049] Wherein, n is any positive integer.

[0050] In some embodiments, the temperature of the third reaction is 30-40°C, preferably 40°C, and the time of the third reaction is 4-6h, preferably 5h.

[0051] Specifically, in this embodiment, 50 ml of acetic acid was added to the intermediate, and the reaction was carried out at 40 degrees Celsius for 5 hours to obtain amylose acetate.

[0052] S2. dissolving the amylose acetate, p-hydroxydiphenol and azelaic acid chloride in a solvent to obtain a mixture;

[0053] In some embodiments, in the mixture, the mass proportion of the amylose acetate is 1%-30%. Preferably, the mass proportion of the amylose acetate is 15%.

[0054] S3. subjecting the mixture to a reflux reaction, followed by acidification, to obtain a chiral liquid crystal polymer. The chiral liquid crystal polymer has the structural formula:

[0055]

[0056] Wherein, m and n are independently selected from positive integers.

[0057] In some embodiments, the acidified acidifying solution comprises hydrochloric acid, and the volume concentration of the hydrochloric acid is 40%-60%. Preferably, the volume concentration of the hydrochloric acid is 50%.

[0058] Specifically, in this embodiment, amylose acetate, p-hydroxydiphenol and azelaic acid chloride are added to a reaction bottle, pyridine is added to dissolve, and the reaction is refluxed for 15 hours. The reaction solution is poured into an appropriate amount of dilute hydrochloric acid solution for acidification, and the solid precipitate is filtered out and washed with a saturated sodium bicarbonate solution and water until neutral, and washed with ethanol several times, and dried in a vacuum drying oven until a constant weight is obtained to obtain a chiral liquid crystal polymer.

[0059] Based on a general inventive concept, an embodiment of the present application further provides a chiral liquid crystal polymer, wherein the chiral liquid crystal polymer is prepared by the preparation method of the chiral liquid crystal polymer provided above.

[0060] The chiral liquid crystal polymer is prepared based on the above method. The specific steps of the method can refer to the above embodiment. Since the chiral liquid crystal polymer adopts part or all of the technical solutions of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment, which will not be repeated here.

[0061] In some embodiments, the chiral liquid crystal polymer has a structural formula of:

[0062]

[0063] Wherein, m and n are independently selected from positive integers.

[0064] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0065] Example 1

[0066] A method for preparing a chiral liquid crystal polymer, the method comprising:

[0067] (1) Synthesis of Amylose Acetate

[0068] 20g of amylose, 20g of tert-butyldimethylsilyl chloride and 100ml of pyridine were added to a reaction bottle and reacted at 10 degrees Celsius for 5 hours. After the reaction, the crude product was evaporated under reduced pressure to obtain a viscous liquid, and then 100ml of acetic anhydride was added and reacted at 95 degrees Celsius for 5 hours. 50ml of acetic acid was added and the temperature was 40 degrees Celsius for 5 hours. After the reaction, the solvent was removed by rotary evaporation, and the crude product was precipitated in methanol to obtain a white powder.

[0069] (2) Synthesis of Liquid Crystal Polymers

[0070] Add 0.5 mol of amylose acetate, 9.5 mol of p-hydroxybiphenol and 10 mmol of azelayl chloride to a three-necked flask, add 50 ml of pyridine to dissolve, heat and react under reflux for 15 hours. Then pour in an appropriate amount of 50% dilute hydrochloric acid solution for acidification, filter the product, wash with alkaline solution, wash with water until neutral, and dry in a vacuum drying oven.

[0071] Example 2

[0072] A method for preparing a chiral liquid crystal polymer, the method comprising:

[0073] (1) Synthesis of Amylose Acetate

[0074] 20g of amylose, 20g of tert-butyldimethylsilyl chloride and 100ml of pyridine were added to a reaction bottle and reacted at 10 degrees Celsius for 5 hours. After the reaction, the crude product was evaporated under reduced pressure to obtain a viscous liquid, and then 100ml of acetic anhydride was added and reacted at 95 degrees Celsius for 5 hours. 50ml of acetic acid was added and the temperature was 40 degrees Celsius for 5 hours. After the reaction, the solvent was removed by rotary evaporation, and the crude product was precipitated in methanol to obtain a white powder.

[0075] (2) Synthesis of Liquid Crystal Polymers

[0076] 1 mol of amylose acetate, 9 mol of p-hydroxybiphenol and 10 mmol of azelayl chloride were added to a three-necked flask, 50 ml of pyridine was added to dissolve, and the mixture was heated under reflux for 15 hours. Then, an appropriate amount of 50% dilute hydrochloric acid solution was added for acidification, and the product was filtered, washed with alkaline solution, washed with water until neutral, and dried in a vacuum drying oven.

[0077] Example 3

[0078] A method for preparing a chiral liquid crystal polymer, the method comprising:

[0079] (1) Synthesis of Amylose Acetate

[0080] 20g of amylose, 20g of tert-butyldimethylsilyl chloride and 100ml of pyridine were added to a reaction bottle and reacted at 10 degrees Celsius for 5 hours. After the reaction, the crude product was evaporated under reduced pressure to obtain a viscous liquid, and then 100ml of acetic anhydride was added and reacted at 95 degrees Celsius for 5 hours. 50ml of acetic acid was added and the temperature was 40 degrees Celsius for 5 hours. After the reaction, the solvent was removed by rotary evaporation, and the crude product was precipitated in methanol to obtain a white powder.

[0081] (2) Synthesis of Liquid Crystal Polymers

[0082] Add 1.5 mol of amylose acetate, 8.5 mol of p-hydroxybiphenol and 10 mmol of azelayl chloride to a three-necked flask, add 50 ml of pyridine to dissolve, heat and react under reflux for 15 hours. Then pour in an appropriate amount of 50% dilute hydrochloric acid solution for acidification, filter the product, wash with alkaline solution, wash with water until neutral, and dry in a vacuum drying oven.

[0083] Example 4

[0084] A method for preparing a chiral liquid crystal polymer, the method comprising:

[0085] (1) Synthesis of Amylose Acetate

[0086] 20g of amylose, 20g of tert-butyldimethylsilyl chloride and 100ml of pyridine were added to a reaction bottle and reacted at 10 degrees Celsius for 5 hours. After the reaction, the crude product was evaporated under reduced pressure to obtain a viscous liquid, and then 100ml of acetic anhydride was added and reacted at 95 degrees Celsius for 5 hours. 50ml of acetic acid was added and the temperature was 40 degrees Celsius for 5 hours. After the reaction, the solvent was removed by rotary evaporation, and the crude product was precipitated in methanol to obtain a white powder.

[0087] (2) Synthesis of Liquid Crystal Polymers

[0088] Add 2 mol of amylose acetate, 8 mol of p-hydroxybiphenol and 10 mmol of azelayl chloride to a three-necked flask, add 50 ml of pyridine to dissolve, heat and react under reflux for 15 hours. Then pour in an appropriate amount of 50% dilute hydrochloric acid solution for acidification, filter the product, wash with alkaline solution, wash with water until neutral, and then dry in a vacuum drying oven.

[0089] Example 5

[0090] A method for preparing a chiral liquid crystal polymer, the method comprising:

[0091] (1) Synthesis of Amylose Acetate

[0092] 20g of amylose, 20g of tert-butyldimethylsilyl chloride and 100ml of pyridine were added to a reaction bottle and reacted at 10 degrees Celsius for 5 hours. After the reaction, the crude product was evaporated under reduced pressure to obtain a viscous liquid, and then 100ml of acetic anhydride was added and reacted at 95 degrees Celsius for 5 hours. 50ml of acetic acid was added and the temperature was 40 degrees Celsius for 5 hours. After the reaction, the solvent was removed by rotary evaporation, and the crude product was precipitated in methanol to obtain a white powder.

[0093] (2) Synthesis of Liquid Crystal Polymers

[0094] Add 2.5 mol of amylose acetate, 7.5 mol of p-hydroxybiphenol and 10 mmol of azelayl chloride to a three-necked flask, add 50 ml of pyridine to dissolve, heat and react under reflux for 15 hours. Then pour in an appropriate amount of 50% dilute hydrochloric acid solution for acidification, filter the product, wash with alkaline solution, wash with water until neutral, and then dry in a vacuum drying oven.

[0095] The polymer materials prepared in Examples 1 to 5 were observed under a polarizing microscope, and it can be seen that the synthesized polymers are inter-conversion thermotropic liquid crystal polymers.

[0096] The properties of the polymer materials prepared in Examples 1 to 5 were analyzed, and the results are shown in the following table:

[0097] TM (Celsius) TG (degrees Celsius) Example 1 300 167 Example 2 280 160 Example 3 258 156 Example 4 237 120 Example 5 213 102

[0098] It can be seen from the above table that, for the polymer material prepared by the examples of the present application, as the content of the chiral monomer amylose increases, the Tg and Tm show a downward trend.

[0099] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0100] In this application, unless otherwise specified, directional words such as "upper" and "lower" used refer specifically to the directions of the drawings in the accompanying drawings. In addition, in the description of the specification of this application, the terms "include", "comprise", etc. mean "including but not limited to".

[0101] In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that there can be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "multiple" refers to two or more. "At least one", "the following at least one (individual)" or similar expressions refer to any combination of these items, including any combination of single (individual) or plural (individual). For example, "at least one (individual) of a, b, or c", or "at least one (individual) of a, b, and c", can all represent: a, b, c, ab (i.e. a and b), ac, bc, or abc, wherein a, b, c can be single or multiple respectively.

[0102] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for preparing a chiral liquid crystal polymer, characterized in that: The method comprises: Obtaining amylose acetate; dissolving the amylose acetate, p-hydroxydiphenol and azelaic acid chloride in a solvent to obtain a mixture; subjecting the mixture to a reflux reaction, and then acidifying it to obtain a chiral liquid crystal polymer; The structural formula of the amylose acetate is: Wherein, n is any positive integer.

2. The method for preparing a chiral liquid crystal polymer according to claim 1, characterized in that: The step of obtaining amylose acetate specifically comprises: Dissolve the amylose and hydroxyl protective agent in a solvent, then perform a first reaction and concentrate to obtain a viscous liquid; The viscous liquid and acetic anhydride are mixed, and then a second reaction is performed to obtain an intermediate; The intermediate is mixed with acetic acid, and then subjected to a third reaction to obtain amylose acetate.

3. The method for preparing a chiral liquid crystal polymer according to claim 2, characterized in that: The hydroxyl protecting agent is tert-butyldimethylsilyl chloride.

4. The method for preparing a chiral liquid crystal polymer according to claim 2, characterized in that: The temperature of the first reaction is 5-15°C; and / or The first reaction time is 4-6 hours.

5. The method for preparing a chiral liquid crystal polymer according to claim 2, characterized in that: The temperature of the second reaction is 90-95°C; and / or The second reaction time is 4-6 hours.

6. The method for preparing a chiral liquid crystal polymer according to claim 2, characterized in that: The temperature of the third reaction is 30-40°C; and / or The time of the third reaction is 4-6h.

7. The method for preparing a chiral liquid crystal polymer according to claim 1, characterized in that: In the mixture, the mass proportion of the amylose acetate is 1%-30%.

8. The method for preparing a chiral liquid crystal polymer according to claim 1, characterized in that: The acidified acidifying solution includes hydrochloric acid, and the volume concentration of the hydrochloric acid is 40%-60%.

9. A chiral liquid crystal polymer, characterized in that: The chiral liquid crystal polymer is prepared by the preparation method of the chiral liquid crystal polymer according to any one of claims 1 to 8.