A biodegradable film and preparation method thereof

By using a combination of PBST, talc, polyethylene glycol and other materials, the biodegradable film is prepared by the tape casting method, which solves the problem of difficulty in balancing production efficiency and thickness uniformity in film processing, and achieves rapid and stable production and high efficiency. Preparation of quality films.

CN116444954BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210011780.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-05
Publication Date
2024-10-15
Estimated Expiration
2042-01-05

AI Technical Summary

Technical Problem

In film processing, the existing technology is difficult to achieve both rapid production and film thickness uniformity in terms of production efficiency and product quality control. Especially when using biodegradable materials, there are problems of slow production speed and uneven thickness.

Method used

A composition consisting of PBST, talc, polyethylene glycol, chain extender and antioxidant is used to prepare a biodegradable film through a casting method. The film is processed through high-speed stirring, twin-screw extrusion and casting equipment to achieve Fast and stable production.

Benefits of technology

The production speed and thickness uniformity of the film are improved, the mechanical properties and stability of the film are improved, a fast and stable production process is achieved, and the preparation cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003457311410000021
    Figure BDA0003457311410000021
  • Figure BDA0003457311410000101
    Figure BDA0003457311410000101
  • Figure QLYQS_1
    Figure QLYQS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of film materials, discloses a biodegradable film and a preparation method thereof, the film is prepared by a composition through a casting method, and the composition is composed of the following raw materials: PBST, talcum powder, polyethylene glycol, optionally a chain extender and optionally an antioxidant; based on the total weight of PBST and talcum powder, the amount of PBST is 85-99 weight %, and the amount of talcum powder is 1-15 weight %; the amount of polyethylene glycol is 2-15% of the total weight of PBST and talcum powder, the amount of chain extender is 0-5% of the total weight of PBST and talcum powder, and the amount of antioxidant is 0-1.5% of the total weight of PBST and talcum powder. The preparation method of the cast film product is simple, low in cost, and has good comprehensive mechanical properties. During processing, the film has good stiffness, uniform film thickness, and stable shape, and rapid and stable production can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of film materials, and in particular, relates to a biodegradable film and a preparation method of the biodegradable film. Background Art

[0002] With the continuous improvement of environmental protection standards, it has become a trend to use more environmentally friendly biodegradable plastics to replace traditional non-degradable plastics, especially in the field of films, such as express packaging films, supermarket shopping bags and other application fields, biodegradable materials have very broad development prospects. Common process types in film processing include cast film, calendering, blow molding and stretching. Cast film production has high efficiency and stable product quality, and is one of the most common methods of all film processing. In the film casting process, speeding up the production speed and optimizing the uniformity of film thickness are of great significance in production efficiency and product quality control. Summary of the invention

[0003] In order to improve production efficiency and product quality, the purpose of the present invention is to provide a biodegradable film and a preparation method thereof, which has the characteristics of fast production speed, stable size, uniform thickness, suitable for rapid production, and the obtained film has good comprehensive performance.

[0004] The first aspect of the present invention provides a biodegradable film, which is prepared from a composition by a casting method, wherein the composition is composed of the following raw materials: PBST, talc, polyethylene glycol, optionally a chain extender and optionally an antioxidant;

[0005] Based on the total weight of PBST and talc, the amount of PBST is 85-99% by weight, the amount of talc is 1-15% by weight; the amount of polyethylene glycol is 2-15% of the total weight of PBST and talc, the amount of chain extender is 0-5% of the total weight of PBST and talc, and the amount of antioxidant is 0-1.5% of the total weight of PBST and talc.

[0006] The second aspect of the present invention provides a method for preparing the above-mentioned biodegradable film, the preparation method comprising:

[0007] 1) adding the raw materials into a high-speed mixer to mix them to obtain a mixed material;

[0008] 2) adding the mixed material into a twin-screw extruder for melting, and then extruding and pelletizing to obtain a composite material;

[0009] 3) Casting the composition in a casting device to obtain the biodegradable film.

[0010] The preparation method of the cast film product of the present invention is simple, low in cost, and has good comprehensive mechanical properties. During the processing, the film has good stiffness, uniform film thickness, and stable shape, and can achieve rapid and stable production.

[0011] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0012] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0013] According to a first aspect of the present invention, the present invention provides a biodegradable film, which is prepared from a composition by a casting method, wherein the composition is composed of the following raw materials: PBST, talc, polyethylene glycol, optionally a chain extender and optionally an antioxidant;

[0014] Based on the total weight of PBST and talc, the amount of PBST is 85-99% by weight, the amount of talc is 1-15% by weight; the amount of polyethylene glycol is 2-15% of the total weight of PBST and talc, the amount of chain extender is 0-5% of the total weight of PBST and talc, and the amount of antioxidant is 0-1.5% of the total weight of PBST and talc.

[0015] In the present invention, the PBST (polybutylene terephthalate-polybutylene succinate copolymer) is a copolymer containing repeating units represented by formula (I) and (II);

[0016]

[0017] In formula (I), m 1 =4,n 1 =2;

[0018] In the PBST, the content of the repeating unit represented by formula (II) is 45-55 mol %.

[0019] According to the present invention, the particle size of the talc powder is 325-8000 mesh, preferably 5000-8000 mesh.

[0020] In the present invention, the molecular weight of the polyethylene glycol is 200-600 g / mol.

[0021] Preferably, based on the total weight of PBST and talc, the amount of PBST is 90-99 weight %, and the amount of talc is 1-10 weight %.

[0022] According to the present invention, the chain extender and antioxidant may be various types conventionally used in the prior art. For example, the antioxidant may be a hindered phenol antioxidant, a phosphite antioxidant, or a pentaerythritol ester antioxidant; the chain extender may be a difunctional acid derivative, an isocyanate, an anhydride, or an epoxide.

[0023] In the present invention, various raw materials can be prepared or commercially available, and the present invention has no particular limitation on their sources, as long as the above-mentioned parameter requirements are met.

[0024] The PBST in the present invention can be prepared by the following method, which specifically comprises the following steps:

[0025] (1) contacting and prepolymerizing a diacid, an ester thereof, an anhydride thereof or a mixture thereof, a diol, and a first catalyst in a reaction vessel under vacuum conditions to obtain a prepolymer; the diacid refers to an organic dicarboxylic acid, such as terephthalic acid and succinic acid; and the diol refers to a primary diol, including butanediol;

[0026] (2) A second catalyst is brought into contact with the prepolymer to perform a vacuum polycondensation reaction to obtain the PBST (polybutylene terephthalate-polybutylene succinate copolymer).

[0027] The present invention has no particular limitation on the mixing order of the components in the reaction system, and the amount of each component used is based on the content of the structural units required by the product.

[0028] According to the present invention, the reaction conditions of each step may also adopt conventional conditions in the art.

[0029] Specifically, in step (1), the reaction conditions of the prepolymerization may include: reaction temperature of 190-250° C.; vacuum degree of 200-600 Pa; reaction time of 1-3 hours, or until the small molecules in the reaction system are almost exhausted and the fraction temperature remains unchanged.

[0030] In step (2), the reaction conditions of the vacuum polycondensation reaction may include: reaction temperature of 200-300° C.; vacuum degree of <300 Pa; and reaction time of 3-12 hours.

[0031] The present invention does not particularly limit the catalyst used in the polymerization reaction and its amount, and can be various conventional catalysts and conventional catalyst amounts for synthesizing polyester. The catalysts used in step (1) and step (2) can be the same or different. For example, the catalyst used in step (1) can be selected from at least one of compounds of metal titanium, antimony and tin; the catalyst used in step (2) can be selected from compounds of rare earth metal Ln and mixtures thereof, wherein the rare earth metal Ln is selected from at least one of lanthanide elements, scandium and yttrium.

[0032] According to the present invention, step (1) and step (2) can be carried out in the same reactor or in different reactors, that is, the prepolymer can be taken out and transferred to another reactor to continue the subsequent polymerization reaction.

[0033] According to the present invention, nitrogen is usually used as protection in the reaction system, but other atmospheres, including air, may also be used.

[0034] According to a second aspect of the present invention, the present invention provides a method for preparing the above-mentioned biodegradable film, the preparation method comprising:

[0035] 1) adding the raw materials into a high-speed mixer to mix them to obtain a mixed material;

[0036] 2) adding the mixed material into a twin-screw extruder for melting, and then extruding and pelletizing to obtain a composite material;

[0037] 3) Casting the composition in a casting device to obtain the biodegradable film.

[0038] The casting device used in the present invention can be conventionally configured according to the prior art. For example, the casting device includes a screw extruder and a casting roller for traction.

[0039] In the present invention, the temperature of the screw extruder (ie, the barrel temperature) may be 80-180° C., and the screw length of the screw extruder may be 20 to 40 times the screw diameter.

[0040] According to the present invention, the temperature of the casting roll can be 20-40° C., and the drawing speed can be any normal drawing speed, preferably 60-80 m / min.

[0041] The substances and parameters not limited in the present invention can be selected according to the existing technology and belong to the conventional technical means in this field.

[0042] The present invention will be further described below with reference to the following examples, but is not limited to these examples.

[0043] In the following examples and comparative examples, the relevant data were obtained according to the following test methods:

[0044] 1. Mechanical properties test: All mechanical properties were tested by Instron 5965 universal testing machine.

[0045] 2. The crystallization temperature of the material is measured by TA's Q-100 DSC. The sample is first isothermally heated at 200°C for 5 minutes to eliminate the thermal history, and then cooled at 10°C / min. The crystallization temperature is calculated according to the peak temperature of the crystallization peak.

[0046] Examples 1-13 are used to illustrate the biodegradable film and the preparation method thereof of the present invention.

[0047] Example 1

[0048] Polybutylene terephthalate-polybutylene succinate copolymer (PBST) and talcum powder are prepared in a weight ratio of 99:1, and then 0.1 weight % of chain extender, 5 weight % of polyethylene glycol, and 0.3 weight % of antioxidant are added to the above materials. The weight percentages of the above chain extender, polyethylene glycol, and antioxidant are calculated based on the sum of the weights of PBST and talcum powder. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Institute of Chemical Industry, and the molar content of repeating unit (II) is 50%. Talc comes from McLean Company, 5000 mesh. The chain extender is from BASF Company ADR 4468. Polyethylene glycol comes from Shanghai Aladdin Biochemical Technology Co., Ltd., with a molecular weight of 600 g / mol. The antioxidant is prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1. The raw materials are first mixed in a high-speed mixer, and the resulting mixture is melted in a twin-screw extruder, and after extrusion and pelletization, a composite is obtained.

[0049] The dried composite pellets were cast using a Collin CR136 E20T casting device, which included a screw extruder and a casting roller for traction. The temperature of the screw extruder was selected within the range of 80-160° C., the temperature of the casting roller was selected at 30° C., and the traction speed was set at 80 m / min.

[0050] Example 2

[0051] Same as Example 1, except that polybutylene terephthalate-polybutylene succinate copolymer (PBST) and talc are prepared in a weight ratio of 95:5.

[0052] Example 3

[0053] Same as Example 1, except that polybutylene terephthalate-polybutylene succinate copolymer (PBST) and talc are prepared in a weight ratio of 90:10; and the pulling speed is adjusted to 60 m / min.

[0054] Example 4

[0055] Same as Example 1, except that polybutylene terephthalate-polybutylene succinate copolymer (PBST) and talc are prepared in a weight ratio of 85:15; and the pulling speed is adjusted to 60 m / min.

[0056] Example 5

[0057] Same as Example 1, except that the particle size of talc is changed to 8000 mesh.

[0058] Example 6

[0059] Same as Example 1, except that the particle size of talc is changed to 2000 mesh.

[0060] Example 7

[0061] Same as Example 1, except that the particle size of talc is changed to 325 mesh.

[0062] Example 8

[0063] Same as Example 1, except that the weight fraction of polyethylene glycol is adjusted to 15%.

[0064] Example 9

[0065] Same as Example 1, except that the weight fraction of polyethylene glycol is adjusted to 2%.

[0066] Example 10

[0067] Same as Example 1, except that the molecular weight of polyethylene glycol is changed to 200 g / mol.

[0068] Embodiment 11

[0069] Same as Example 1, except that the molecular weight of polyethylene glycol is changed to 400 g / mol.

[0070] Example 12

[0071] Same as Example 1, except that the molar content of the repeating unit (II) in the polybutylene terephthalate-polybutylene succinate copolymer (PBST) is 45%.

[0072] Embodiment 13

[0073] Same as Example 1, except that the molar content of the repeating unit (II) in the polybutylene terephthalate-polybutylene succinate copolymer (PBST) is 55%.

[0074] Comparative Example 1

[0075] Take polybutylene terephthalate-polybutylene succinate copolymer (PBST) material, add 0.1 wt% chain extender and 0.3 wt% antioxidant to the material. The weight percentages of the chain extender and antioxidant are calculated based on the weight of PBST. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Chemical Research Institute, and the molar content of repeating unit (II) is 50%. The chain extender is BASF's ADR4468. The antioxidant is prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1. The raw materials are first mixed in a high-speed mixer, and the resulting mixture is melted in a twin-screw extruder, and then extruded and pelletized to obtain a composite.

[0076] The dried composite pellets were cast using a Collin CR136 E20T casting device, which included a screw extruder and a casting roller for traction. The temperature of the screw extruder was selected within the range of 80-160° C., the temperature of the casting roller was selected at 30° C., and the traction speed was set at 80 m / min.

[0077] Comparative Example 2

[0078] Take polybutylene terephthalate-polybutylene succinate copolymer (PBST) material, add 0.1 wt% chain extender, 5 wt% polyethylene glycol, and 0.3 wt% antioxidant to the material. The weight percentages of the chain extender, polyethylene glycol, and antioxidant are all calculated based on the weight of PBST. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Chemical Research Institute, and the molar content of repeating unit (II) is 50%. The chain extender is BASF's ADR 4468. Polyethylene glycol comes from Shanghai Aladdin Biochemical Technology Co., Ltd., with a molecular weight of 600 g / mol. The antioxidant is prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1. The raw materials are first mixed in a high-speed mixer, and the resulting mixture is melted in a twin-screw extruder, and after extrusion and pelletization, a composite is obtained.

[0079] The dried composite pellets were cast using a Collin CR136 E20T casting device, which included a screw extruder and a casting roller for traction. The temperature of the screw extruder was selected within the range of 80-160° C., the temperature of the casting roller was selected at 30° C., and the traction speed was set at 80 m / min.

[0080] Comparative Example 3

[0081] Polybutylene terephthalate-polybutylene succinate copolymer (PBST) and talcum powder are prepared in a weight ratio of 99:1, and then 0.1% by weight of a chain extender and 0.3% by weight of an antioxidant are added to the above materials. The weight percentages of the above chain extender and antioxidant are calculated based on the sum of the weights of PBST and talcum powder. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Institute of Chemical Industry, and the molar content of repeating unit (II) is 50%. Talc powder comes from Maclean Company, 5000 mesh. The chain extender is from BASF Company ADR 4468. The antioxidant was prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1. The raw materials were first mixed in a high-speed mixer, and the resulting mixture was melted in a twin-screw extruder, and extruded and pelletized to obtain a composite.

[0082] The dried composite pellets were cast using a Collin CR136E20T casting device, which included a screw extruder and a casting roller for traction. The temperature of the screw extruder was selected within the range of 80-160° C., the temperature of the casting roller was selected at 30° C., and the traction speed was set at 80 m / min.

[0083] Comparative Example 4

[0084] Polybutylene terephthalate-polybutylene succinate copolymer (PBST) and talcum powder are prepared in a weight ratio of 80:20, and then 0.1 weight % of chain extender, 5 weight % of polyethylene glycol, and 0.3 weight % of antioxidant are added to the above materials. The weight percentages of the above chain extender, polyethylene glycol, and antioxidant are calculated based on the sum of the weights of PBST and talcum powder. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Institute of Chemical Industry, and the molar content of repeating unit (II) is 50%. Talc comes from McLean Company, 5000 mesh. The chain extender is from BASF Company ADR 4468. Polyethylene glycol comes from Shanghai Aladdin Biochemical Technology Co., Ltd., with a molecular weight of 600 g / mol. The antioxidant is prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1. The raw materials are first mixed in a high-speed mixer, and the resulting mixture is melted in a twin-screw extruder, and after extrusion and pelletization, a composite is obtained.

[0085] The dried composite pellets were cast using a Collin CR136 E20T casting device, which included a screw extruder and a casting roller for traction. The temperature of the screw extruder was selected within the range of 80-160° C., the temperature of the casting roller was selected at 30° C., and the traction speed was set at 80 m / min.

[0086] Comparative Example 5

[0087] Polybutylene terephthalate-polybutylene succinate copolymer (PBST) and talcum powder are prepared in a weight ratio of 99:1, and then 0.1 weight % of chain extender, 5 weight % of glycerol, and 0.3 weight % of antioxidant are added to the above materials. The weight percentages of the above chain extender, glycerol, and antioxidant are calculated based on the sum of the weights of PBST and talcum powder. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Chemical Research Institute, and the molar content of repeating unit (II) is 50%. Talc comes from McLean Company, 5000 mesh. The chain extender is from BASF Company ADR 4468. Glycerol was obtained from Shanghai Aladdin Biochemical Technology Co., Ltd. The antioxidant was prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1. The raw materials were first mixed in a high-speed mixer, and the resulting mixture was melted in a twin-screw extruder, and extruded and pelletized to obtain a composite.

[0088] The dried composite pellets were cast using a Collin CR136E20T casting device, which included a screw extruder and a casting roller for traction. The temperature of the screw extruder was selected within the range of 80-160° C., the temperature of the casting roller was selected at 30° C., and the traction speed was set at 80 m / min.

[0089] The production conditions of the films of various embodiments and comparative examples and the properties of the films obtained are shown in Table 1.

[0090] Table 1

[0091]

[0092] Note: MD stands for machine direction and TD stands for transverse direction.

[0093] As can be seen from Table 1, the addition of talcum powder in the film of the present invention can greatly increase the crystallization temperature of PBST by up to 20°C or more, so the crystallization solidification rate of the melt can be significantly increased, the production speed can be accelerated, and the stability of the film can be improved at the same time. The thickness of the obtained film is uniform, and the films are not easy to stick together. In addition, the addition of talcum powder can also improve the mechanical strength of PBST film products and significantly improve the processing rate. There is a range for the content and particle size of talcum powder, within which rapid processing and film stability can be met, and the obtained film has a good balance of rigidity and toughness. Beyond this range, the above characteristics are not possessed. The function of polyethylene glycol is to significantly improve the elongation at break of the material, so that the film has good toughness, is not easy to break, and is easy to prepare a thinner film; at the same time, a higher production speed can be achieved. It can be seen that within the required composition range, the material has a good balance of rigidity and toughness.

[0094] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

Claims

1. A biodegradable film, characterized in that: The film is prepared from a composition by a casting method, wherein the composition is composed of the following raw materials: PBST, talcum powder, polyethylene glycol, a chain extender and an antioxidant; Based on the total weight of PBST and talc, the amount of PBST is 85-99% by weight, and the amount of talc is 1-15% by weight; the amount of polyethylene glycol is 2-15% of the total weight of PBST and talc, the amount of chain extender is 0.1-5% of the total weight of PBST and talc, and the amount of antioxidant is 0.3-1.5% of the total weight of PBST and talc; The PBST is a copolymer containing repeating units represented by formula (I) and (II); Formula (I) Formula (II) In formula (I), m1=4, n1=2; In the PBST, the content of the repeating unit represented by formula (II) is 45-55 mol%; The particle size of the talcum powder is 325-8000 mesh; The molecular weight of the polyethylene glycol is 200-600 g / mol.

2. The biodegradable film according to claim 1, wherein: The particle size of the talcum powder is 5000-8000 mesh.

3. The biodegradable film according to claim 1, wherein: Based on the total weight of PBST and talc, the amount of PBST used is 90-99 weight %, and the amount of talc used is 1-10 weight %.

4. The method for preparing a biodegradable film according to any one of claims 1 to 3, characterized in that: The preparation method comprises: 1) Adding various raw materials into a high-speed mixer to mix them to obtain a mixed material; 2) adding the mixed material into a twin-screw extruder for melting, and obtaining a composite material after extrusion and pelletization; 3) Casting the composition in a casting device to obtain the biodegradable film.

5. The method for preparing a biodegradable film according to claim 4, wherein: The casting equipment includes a screw extruder and a casting roll for drawing.

6. The method for preparing a biodegradable film according to claim 5, wherein: The temperature of the screw extruder is 80-180°C.

7. The method for preparing a biodegradable film according to claim 5, wherein: The temperature of the casting roll is 20-40°C, and the pulling speed is 60-80m / min.