High-mobility n-type thin film assembled vertically with nano-diamond sheets and preparation method thereof
Through chemical vapor deposition and microwave plasma treatment, a high mobility nanodiamond sheet vertical assembly structure was prepared, which solved the problem of low conductivity of diamond films in the prior art, and achieved a high mobility and high conductivity nanodiamond film. , suitable for electronic devices and electrochemical electrodes.
Patent Information
- Application Number
- CN202310203923.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-03-06
AI Technical Summary
The prior art is difficult to prepare n-type diamond films with low resistivity and high mobility, especially in nano-sized diamond films. The presence of an amorphous carbon phase leads to low conductivity and is difficult to apply to electronic devices and electrochemical electrodes.
Nanodiamond/graphite composite vertical sheet film was prepared by chemical vapor deposition method, and the microwave argon/oxygen mixed plasma was used to form a high mobility nanodiamond sheet vertical assembly structure.
The n-type carrier mobility with high mobility is achieved, which simplifies process operations and improves the conductive properties of the film, with a larger specific surface area and unique application advantages.
Smart Images

Figure HDA0004110063190000011 
Figure HDA0004110063190000012 
Figure HDA0004110063190000021
Abstract
Description
Technical Field
[0001] The invention relates to a high-mobility n-type thin film of vertically assembled nano diamond sheets and a preparation method thereof. Background Art
[0002] Diamond has a very wide bandgap, which makes it a new generation of semiconductor materials after silicon, germanium and other materials, and has broad application prospects in optoelectronics, electrochemistry, semiconductors and other high-tech fields. However, diamond has not been used in the microelectronics industry. The key reason is that it is difficult to prepare n-type diamond with low resistivity and high mobility to make prototype devices such as pn junctions. Over the years, many researchers have tried to dope impurity elements into single crystal diamond and microcrystalline diamond films in the hope of obtaining n-type diamond films with high conductivity, but good results have not been achieved. The doped diamond film has low conductivity and low electron mobility, making it difficult to use as an electronic device.
[0003] Nano-sized diamond grains have small size effects and surface effects, which make nano-diamond films have better doping potential than microcrystalline and single-crystal diamond films. However, traditional nano-diamond films contain a large amount of amorphous carbon phase, which reduces the conductivity of the film. In order to solve this problem, we invented a film with a novel grain dense packing structure in the authorized patents ZL201810247215.1 and ZL20181025815.4. The interface is formed between the nano-diamond grains, there is no amorphous carbon, and it exhibits high-mobility n-type conductivity. However, the above-mentioned continuous dense packing structure exists in the film. If the dense packing structure can be prepared into nano-vertical sheets with a larger specific surface area, it may have unique application advantages in electrical devices, electrochemical electrodes, etc. Summary of the invention
[0004] The purpose of the present invention is to prepare a high mobility n-type film with a close-packed structure of nano-diamond vertical sheets. A nano-diamond / graphite composite vertical sheet film is prepared by a chemical vapor deposition method, and then treated by a mixed plasma of argon and oxygen to prepare a diamond film with a three-dimensional structure of nano-diamond sheets vertically assembled and high n-type carrier mobility.
[0005] To achieve the above object, the present invention adopts the following technical solution:
[0006] The present invention provides a high-mobility n-type thin film formed by vertically assembling nano-diamond sheets. The high-mobility n-type thin film formed by vertically assembling nano-diamond sheets is prepared by the following method:
[0007] (1) Pretreatment of single crystal silicon substrate surface grinding and seeding: diamond powder and glycerol are fully dispersed and mixed to obtain a diamond grinding paste; the diamond grinding paste is taken on a polishing flannel cloth, and an intrinsic single crystal silicon wafer is pressed back and forth on the grinding paste for 5 to 40 minutes (preferably 30 minutes); the polished silicon wafer is ultrasonically cleaned in acetone and anhydrous ethanol for 1 to 30 minutes (preferably 5 minutes), and dried with nitrogen to obtain a single crystal silicon after seeding;
[0008] (2) Hot Wire Chemical Vapor Deposition Thin Film Growth: The seeded single crystal silicon described in step (1) is placed as a substrate in a hot wire chemical vapor deposition device, and acetone is used as a carbon source. The acetone is introduced into the reaction chamber by bubbling hydrogen at a flow rate of 70-110 sccm (preferably 90 sccm). Pure hydrogen at a flow rate of 100-300 sccm (preferably 200 sccm) is also introduced. The growth power is controlled to be 2000-2600 W (preferably 2200 W) and the growth pressure is controlled to be 1.0-2.5 kPa (preferably 1.6 kPa) to grow a nano-diamond particle layer for 10-50 m in (preferably 20 min); adjust the pure hydrogen flow rate to 0-20 sccm (preferably 0 sccm), the hydrogen flow rate (i.e., acetone flow rate) to 50-100 sccm (preferably 100 sccm), reduce the power to 1300-1800 W (preferably 1800 W), and grow the vertical nano-diamond / graphene composite sheet for 0.5-10 min (preferably 3 min); stop passing the pure hydrogen and acetone, and slowly reduce the power to 0 at a rate of 0.1-5 V / min (preferably 0.5 V / min) to obtain a silicon wafer containing vertical nano-diamond / graphene composite sheets;
[0009] (3) Microwave argon / oxygen mixed plasma etching treatment: Place the silicon wafer containing the vertical nanodiamond / graphene composite sheet layer described in step (2) in a microwave plasma vapor deposition device, and introduce a mixed plasma of argon and oxygen, wherein the total flow rate of argon and oxygen is 80-120 sccm (preferably 100 sccm), and the flow rate of oxygen in the mixed plasma is controlled to be 10-20 sccm (preferably 10 sccm); control the power to 400-800 W (preferably 600 W), the gas pressure to 10-20 Torr (preferably 15 Torr), and the processing time to 2-8 min (preferably 4 min), to obtain a high-mobility n-type thin film with vertical assembly of the nanodiamond sheets.
[0010] Among them, the oxygen flow rate is crucial to the carrier mobility of the high-mobility n-type thin film assembled vertically by the nano-diamond sheets of the present invention. Too low mobility will greatly reduce, and too high mobility will also weaken.
[0011] Furthermore, the diamond powder described in step (1) has a particle size of 500 nm and is purchased from Zhecheng Huifeng Diamond Technology Co., Ltd. in one embodiment of the present invention.
[0012] Furthermore, in step (1), the present invention recommends that the diamond powder and glycerol be fully dispersed and mixed by ultrasonic dispersion for 10 to 30 minutes, and in one embodiment of the present invention, for 20 minutes.
[0013] Furthermore, the volume of the glycerol in step (1) is 50-150 mL / g (preferably 90-110 mL / g, particularly preferably 100 mL / g) based on the mass of the diamond powder.
[0014] Further, in one embodiment of the present invention, the intrinsic single crystal silicon wafer in step (1) is a single-sided polished silicon wafer of Zhejiang Lijing Optoelectronics Technology, with a thickness of 500±10μm, a diameter of 100±0.4mm, a resistivity of 0.011-0.01Ωcm, and a model / crystal orientation: P <100> .
[0015] The present invention particularly recommends that the high mobility n-type thin film of the vertically assembled nano-diamond sheets be prepared by the following method:
[0016] (1) Pretreatment of single crystal silicon substrate surface grinding and seeding: diamond powder and glycerol are fully dispersed and mixed to obtain diamond grinding paste; the diamond grinding paste is taken on a polishing flannel cloth, and an intrinsic single crystal silicon wafer is pressed back and forth on the grinding paste for 30 minutes. The polished silicon wafer is ultrasonically cleaned in acetone and anhydrous ethanol for 5 minutes in turn, and dried with nitrogen to obtain single crystal silicon after seeding;
[0017] The volume of the glycerol is 100 mL / g based on the mass of the diamond powder;
[0018] (2) Hot wire chemical vapor deposition thin film growth: the single crystal silicon after seeding described in step (1) is placed as a substrate in a hot wire chemical vapor deposition device, acetone is used as a carbon source, and the acetone is introduced into the reaction chamber by bubbling hydrogen with a flow rate of 90 sccm. At the same time, a flow rate of 200 sccm is introduced, and the growth power is controlled to be 2200 W and the growth pressure is 1.6 kPa to grow a nano-diamond particle layer for 20 minutes; the pure hydrogen flow rate is adjusted to 0 sccm and the hydrogen flow rate is 100 sccm, and the power is reduced to 1800 W to grow a vertical nano-diamond / graphene composite layer for 3 minutes; the introduction of pure hydrogen and acetone is stopped, and the power is slowly reduced to 0 at 0.5 V / min to obtain a silicon wafer containing a vertical nano-diamond / graphene composite layer;
[0019] (3) Microwave argon / oxygen mixed plasma etching treatment: The silicon wafer containing the vertical nanodiamond / graphene composite sheet layer described in step (2) is placed in a microwave plasma vapor deposition device, and a mixed plasma of argon and oxygen is introduced, wherein the total flow rate of argon and oxygen is 100 sccm, and the flow rate of oxygen in the mixed plasma is controlled to be 10 sccm; the power is controlled to be 600 W, the gas pressure is 15 Torr, and the processing time is 4 min, to obtain a high-mobility n-type thin film with vertical assembly of the nanodiamond sheets.
[0020] Compared with the prior art, the beneficial effects of the present invention are mainly reflected in: 1. It adopts microwave plasma chemical vapor deposition equipment for treatment, the process is simple and easy to operate, and the obtained nano diamond is in the form of upright sheets; 2. The prepared nano diamond sheet has a higher n-type carrier mobility. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Field emission scanning electron microscope (FESEM) image of NCD-10 sample with oxygen content of 10 sccm;
[0022] Figure 2 Visible Raman spectrum (Raman) of NCD-10 sample with oxygen content of 10 sccm;
[0023] Figure 3 This is a high-resolution transmission electron microscopy (HRTEM) image of the NCD-10 sample with an oxygen content of 10 sccm;
[0024] Figure 4 FESEM image of NCD-15 sample with oxygen content of 15 sccm;
[0025] Figure 5 is the Raman spectrum of the NCD-15 sample with an oxygen content of 15 sccm;
[0026] Figure 6 HRTEM image of NCD-15 sample with oxygen content of 15 sccm;
[0027] Figure 7 FESEM image of NCD-20 sample with oxygen content of 20 sccm;
[0028] Figure 8 is the Raman spectrum of the NCD-20 sample with an oxygen content of 20 sccm;
[0029] Fig. 9 HRTEM image of NCD-20 sample with oxygen content of 20 sccm; DETAILED DESCRIPTION
[0030] The present invention is further described below by means of specific embodiments, but the protection scope of the present invention is not limited thereto.
[0031] Example 1
[0032] Diamond powder (Zhecheng Huifeng Diamond Technology Co., Ltd., particle size 500nm) and glycerol (glycerol) were mixed in a ratio of 1g:100ml, and ultrasonically dispersed for 20min to obtain diamond grinding paste; the diamond grinding paste was taken on a polishing flannel cloth and pressed on an intrinsic single crystal silicon wafer (Zhejiang Lijing Optoelectronics Technology, single-sided polished silicon wafer, thickness 500±10μm, diameter 100±0.4mm, resistivity 0.011-0.01Ωcm, model / crystal orientation: P <100> ) was polished back and forth at the grinding paste for 30 minutes, and the treated silicon wafer was ultrasonically cleaned in acetone and anhydrous ethanol for 5 minutes, and dried with nitrogen to obtain single crystal silicon after seeding; the single crystal silicon after seeding was placed in a hot wire chemical vapor deposition device as a substrate, and acetone was used as a carbon source. The acetone was introduced into the reaction chamber by bubbling hydrogen with a flow rate of 90sccm, and pure hydrogen with a flow rate of 200sccm was also introduced. The growth power was controlled to be 2200W and the growth pressure was 1.6kPa to grow the nano diamond particle layer for 20 minutes; the pure hydrogen flow rate was adjusted to 0sccm, the acetone flow rate was 100sccm, and the power was reduced to 180 0W, growing the vertical nano-diamond / graphene composite sheet for 3 minutes; stopping the introduction of acetone, and slowly reducing the power to 0 at a rate of 0.5V / min to obtain a silicon wafer containing the vertical nano-diamond / graphene composite sheet; placing the silicon wafer with the vertical nano-diamond / graphene composite sheet in a microwave plasma vapor deposition device, and introducing argon and oxygen mixed plasma, wherein the total flow rate of argon and oxygen is 100sccm; controlling the power to 600W, the gas pressure to 15Torr, the processing time to 4min, and controlling the oxygen flow rate in the plasma to 10sccm, to obtain a high-mobility n-type thin film with vertical assembly of the nano-diamond sheets.
[0033] The surface morphology of the film was observed by field emission scanning electron microscopy; the phase composition of the sample was detected by visible light Raman spectroscopy; the microstructure composition inside the sample was analyzed by high-resolution transmission analysis; and the electrical properties of the film were tested by Hall effect tester.
[0034] Figure 1 This is a FESEM photo of a NCD-10 sample with an oxygen content of 10 sccm at 50,000 times magnification. It can be seen that a significant lamellar structure is distributed on the surface of a single particle, with a thickness of about 1.04 μm. The particle is etched, and the lamellar structure on the surface is relatively complete.
[0035] Figure 2 Raman spectrum of NCD-10 sample with oxygen content of 10 sccm. 2200-3500cm -1The peak of the band basically disappeared, indicating that the graphite component was severely etched. -1 The very weak absorption peak at 1332cm -1 A weaker diamond peak appeared.
[0036] Figure 3 This is the HRTEM image of the NCD-10 sample with an oxygen content of 10 sccm. From the overall selected area electron diffraction (SAED) image, it can be seen that the outer circle is a bright nanodiamond diffraction ring, and there is a small amount of dispersed graphite and amorphous phase signals inside, indicating that the sample is composed of nanodiamond phase and a small amount of graphite / amorphous phase, which is consistent with the results in the Raman spectrum. Combined with the FESEM photo, it can be determined to be a nanodiamond sheet structure. When the local area is magnified and Fourier diffraction transform analysis is performed, clear diffraction spots of nanodiamond can be seen, and obvious nanodiamond diffraction stripes can be seen in the enlarged image, that is, the sample is mainly a sheet structure built by small-sized nanodiamond grains.
[0037] The Hall effect electrical test of NCD-10 sample with oxygen content of 10 sccm shows that the carrier mobility of the sample is 845 cm 2 V -1 s -1 , and belongs to n-type conductivity.
[0038] Example 2
[0039] Diamond powder (Zhecheng Huifeng Diamond Technology Co., Ltd., particle size 500nm) and glycerol (glycerol) were mixed in a ratio of 1g:100ml, and ultrasonically dispersed for 20min to obtain diamond grinding paste; the diamond grinding paste was taken on a polishing flannel cloth and pressed on an intrinsic single crystal silicon wafer (Zhejiang Lijing Optoelectronics Technology, single-sided polished silicon wafer, thickness 500±10μm, diameter 100±0.4mm, resistivity 0.011-0.01Ωcm, model / crystal orientation: P <100> ) was polished back and forth at the grinding paste for 30 minutes, and the treated silicon wafer was ultrasonically cleaned in acetone and anhydrous ethanol for 5 minutes, and dried with nitrogen to obtain single crystal silicon after seeding; the single crystal silicon after seeding was placed in a hot wire chemical vapor deposition device as a substrate, and acetone was used as a carbon source. The acetone was introduced into the reaction chamber by bubbling hydrogen with a flow rate of 90sccm, and pure hydrogen with a flow rate of 200sccm was also introduced. The growth power was controlled to be 2200W and the growth pressure was 1.6kPa to grow the nano diamond particle layer for 20 minutes; the pure hydrogen flow rate was adjusted to 0sccm, the acetone flow rate was 100sccm, and the power was reduced to 180 0W, growing the vertical nano-diamond / graphene composite layer for 3 minutes; stopping the introduction of acetone, and slowly reducing the power to 0 at a rate of 0.5V / min to obtain a silicon wafer containing the vertical nano-diamond / graphene composite layer; placing the silicon wafer with the vertical nano-diamond / graphene composite layer in a microwave plasma vapor deposition device, and introducing argon and oxygen mixed plasma, wherein the total flow rate of argon and oxygen is 100sccm; controlling the power to 600W, the gas pressure to 15Torr, the processing time to 4min, and controlling the oxygen flow rate in the plasma to 15sccm, to obtain a high-mobility n-type thin film with vertical assembly of the nano-diamond sheets.
[0040] The surface morphology of the film was observed by field emission scanning electron microscopy; the phase composition of the sample was detected by visible light Raman spectroscopy; the microstructure composition inside the sample was analyzed by high-resolution transmission analysis; and the electrical properties of the film were tested by Hall effect tester.
[0041] Figure 4 This is a FESEM photo of a NCD-15 sample with an oxygen content of 15 sccm at 50,000 times magnification. Lamellar collapse begins to appear on the top of the particle, and the cross-sectional thickness continues to decrease (0.90 μm), while the lamellae at the edge of the particle are still relatively intact.
[0042] Figure 5 This is the Raman spectrum of the NCD-15 sample with an oxygen content of 15 sccm. 2200-3500cm -1 The peak of the band basically disappeared, indicating that the graphite component was severely etched. Compared with the NCD-10 sample, the 1332cm -1The diamond peak at 40° becomes more prominent, and the half-peak width of the G peak increases slightly, indicating that the ordering degree and size of the graphite clusters gradually decrease. Therefore, under the action of plasma with an oxygen content of 15 sccm, the graphite component of the film is very small, showing that the film component is mainly nanodiamond.
[0043] Figure 6 This is the HRTEM image of the NCD-15 sample with an oxygen content of 15 sccm. The SAED image shows polycrystalline diffraction rings of diamond, indicating that when the oxygen flow rate is 15 sccm, due to the etching effect of strong oxygen, the graphite phase and amorphous phase inside the film are reduced, which is consistent with the results in the Raman spectrum. When the local area is magnified and Fourier diffraction transform analysis is performed, obvious diamond (111) diffraction rings are displayed, indicating that the position is mainly composed of diamond grains. The inset shows a diamond fringe spacing of 0.208nm, and there is no graphite layer covering the periphery of the grains, that is, at this time the sample is mainly a lamellar structure composed of nano-diamond grains.
[0044] The Hall effect electrical test of NCD-15 sample with oxygen content of 15 sccm shows that the carrier mobility of the sample is 497.46 cm 2 V -1 s -1 , and belongs to n-type conductivity.
[0045] Example 3
[0046] Diamond powder (Zhecheng Huifeng Diamond Technology Co., Ltd., particle size 500nm) and glycerol (glycerol) were mixed in a ratio of 1g:100ml, and ultrasonically dispersed for 20min to obtain diamond grinding paste; the diamond grinding paste was taken on a polishing flannel cloth and pressed on an intrinsic single crystal silicon wafer (Zhejiang Lijing Optoelectronics Technology, single-sided polished silicon wafer, thickness 500±10μm, diameter 100±0.4mm, resistivity 0.011-0.01Ωcm, model / crystal orientation: P <100> ) was polished back and forth at the grinding paste for 30 minutes, and the treated silicon wafer was ultrasonically cleaned in acetone and anhydrous ethanol for 5 minutes, and dried with nitrogen to obtain single crystal silicon after seeding; the single crystal silicon after seeding was placed in a hot wire chemical vapor deposition device as a substrate, and acetone was used as a carbon source. The acetone was introduced into the reaction chamber by bubbling hydrogen with a flow rate of 90sccm, and pure hydrogen with a flow rate of 200sccm was also introduced. The growth power was controlled to be 2200W and the growth pressure was 1.6kPa to grow the nano diamond particle layer for 20 minutes; the pure hydrogen flow rate was adjusted to 0sccm, the acetone flow rate was 100sccm, and the power was reduced to 180 0W, growing the vertical nano-diamond / graphene composite layer for 3 minutes; stopping the introduction of acetone, and slowly reducing the power to 0 at a rate of 0.5V / min to obtain a silicon wafer containing the vertical nano-diamond / graphene composite layer; placing the silicon wafer with the vertical nano-diamond / graphene composite layer in a microwave plasma vapor deposition device, and introducing argon and oxygen mixed plasma, wherein the total flow rate of argon and oxygen is 100sccm; controlling the power to 600W, the gas pressure to 15Torr, the processing time to 4min, and controlling the oxygen flow rate in the plasma to 20sccm, to obtain a high-mobility n-type thin film with vertical assembly of the nano-diamond sheets.
[0047] The surface morphology of the film was observed by field emission scanning electron microscopy; the phase composition of the sample was detected by visible light Raman spectroscopy; the microstructure composition inside the sample was analyzed by high-resolution transmission analysis; and the electrical properties of the film were tested by Hall effect tester.
[0048] Figure 7 This is a FESEM photo of a NCD-20 sample with an oxygen content of 20 sccm at 50,000 times. The lamellae on the top of the particle are severely collapsed, and a small amount of lamellae structure is still retained at the edge. The film thickness in the cross-sectional view is 0.86 μm.
[0049] Figure 8 This is the Raman spectrum of the NCD-20 sample with an oxygen content of 20 sccm. The spectrum shows 2000-3500 cm -1 The peak of the band basically disappeared, indicating that the graphite component was greatly reduced. The diamond peak continued to maintain a sharp peak shape, and the half-peak width of the G peak continued to increase, indicating that the graphite component of the film continued to decrease under the action of the plasma with an oxygen content of 20 sccm, showing a structure dominated by nanodiamonds.
[0050] Fig. 9 This is the HRTEM image of the NCD-20 sample with an oxygen content of 20 sccm. The SAED image shows polycrystalline diffraction rings of diamond (111), (220) and (311) planes, and several sharp bright spots appear on the rings, indicating that there are relatively large particles of nanodiamonds in the structure, and graphite and amorphous phases are not obviously present, which is consistent with the results in the Raman spectrum. When the local area is magnified and Fourier diffraction transform analysis is performed, clear diffraction spots of nanodiamonds can be seen, and the enlarged image shows obvious nanodiamond diffraction stripes with a spacing of 0.208nm, that is, at this time, the sample is mainly a layered structure built by relatively large particles of nanodiamonds (size>10nm).
[0051] The Hall effect electrical test of NCD-20 sample with oxygen content of 20 sccm shows that the carrier mobility of the sample is 667.88 cm 2 V -1 s -1 , and belongs to n-type conductivity.
[0052] Comparative Example 1
[0053] The experimental conditions were consistent with those in Example 1, with the only difference being that the flow rate of oxygen in the plasma gas was changed to 0 sccm. The nanodiamond / graphene composite vertical lamellae film was obtained, and the carrier mobility of the sample was 7.20 cm 2 V -1 s -1 , and belongs to n-type conductivity.
[0054] Comparative Example 2
[0055] The experimental conditions were consistent with those in Example 2, with the only difference being that the flow rate of oxygen in the plasma gas was changed to 2 sccm. The nanodiamond / graphene composite vertical lamellae film was obtained, and the carrier mobility of the sample was 106.20 cm 2 V -1 s -1 , and belongs to n-type conductivity.
[0056] Comparative Example 3
[0057] The experimental conditions were consistent with those in Example 3, with the only difference being that the flow rate of oxygen in the plasma gas was changed to 5 sccm. The nanodiamond / graphene composite vertical lamellae film was obtained, and the carrier mobility of the sample was 1.95 cm 2 V -1 s -1 , and belongs to n-type conductivity.
Claims
1. A high mobility n-type thin film composed of vertically assembled nano-diamond sheets, characterized in that The high mobility n-type thin film assembled vertically from the nano-diamond sheets is prepared as follows: (1) Pretreatment of single crystal silicon substrate surface grinding and seeding: diamond powder and glycerol are fully dispersed and mixed to obtain diamond grinding paste; the diamond grinding paste is taken on a polishing flannel cloth, and an intrinsic single crystal silicon wafer is pressed back and forth on the grinding paste for 5 to 40 minutes. The polished silicon wafer is ultrasonically cleaned in acetone and anhydrous ethanol for 1 to 30 minutes, and dried with nitrogen to obtain single crystal silicon after seeding; (2) growing a thin film by hot wire chemical vapor deposition: placing the seeded single crystal silicon described in step (1) as a substrate into a hot wire chemical vapor deposition device, using acetone as a carbon source, and introducing the acetone into the reaction chamber by bubbling hydrogen at a flow rate of 70-110 sccm, while also introducing pure hydrogen at a flow rate of 100-300 sccm, controlling the growth power to 2000-2600 W, and the growth pressure to 1.0-2.5 kPa to grow a nano-diamond particle layer for 10-50 min; adjusting the pure hydrogen flow rate to 0-20 sccm, the hydrogen flow rate to 50-100 sccm, reducing the power to 1300-1800 W, and growing a vertical nano-diamond / graphene composite layer for 0.5-10 min; stopping the introduction of pure hydrogen and acetone, and slowly reducing the power to 0 at a rate of 0.1-5 V / min to obtain a silicon wafer containing a vertical nano-diamond / graphene composite layer; (3) Microwave argon / oxygen mixed plasma etching treatment: The silicon wafer containing the vertical nano-diamond / graphene composite sheet layer described in step (2) is placed in a microwave plasma vapor deposition device, and a mixed plasma of argon and oxygen is introduced, wherein the total flow rate of argon and oxygen is 80 to 120 sccm, and the flow rate of oxygen in the mixed plasma is controlled to be 10 to 20 sccm; the power is controlled to be 400 to 800 W, the gas pressure is 10 to 20 Torr, and the processing time is 2 to 8 min, to obtain a high-mobility n-type thin film with vertical assembly of the nano-diamond sheets.
2. The high-mobility n-type thin film of vertically assembled nano-diamond sheets as claimed in claim 1, characterized in that: The particle size of the diamond powder described in step (1) is 500 nm.
3. The high-mobility n-type thin film of vertically assembled nano-diamond sheets as claimed in claim 1, characterized in that: The intrinsic single crystal silicon wafer in step (1) is a single-sided polished silicon wafer from Zhejiang Lijing Optoelectronics Technology Co., Ltd., with a thickness of 500±10μm, a diameter of 100±0.4mm, a resistivity of 0.011-0.01Ωcm, and a model / crystal orientation: P <100> .
4. The high-mobility n-type thin film of vertically assembled nanodiamond sheets as claimed in claim 1, characterized in that: The volume of the glycerol in step (1) is 50-150 mL / g based on the mass of the diamond powder.
5. The high-mobility n-type thin film of vertically assembled nano-diamond sheets as claimed in claim 1, characterized in that: In step (2), the acetone is introduced into the reaction chamber by bubbling hydrogen at a flow rate of 90 sccm, and pure hydrogen at a flow rate of 200 sccm is also introduced.
6. The high-mobility n-type thin film of vertically assembled nano-diamond sheets as claimed in claim 1, characterized in that: In step (2), the growth power is 2200 W, the growth pressure is 1.6 kPa, and the growth time is 20 min.
7. The high-mobility n-type thin film of vertically assembled nano-diamond sheets as claimed in claim 1, characterized in that: The total flow rate of argon and oxygen in step (3) is 100 sccm.
8. The high-mobility n-type thin film of vertically assembled nano-diamond sheets as claimed in claim 1, characterized in that: The flow rate of oxygen in step (3) is 10 sccm.
9. The high-mobility n-type thin film of vertically assembled nano-diamond sheets as claimed in claim 1, characterized in that: In step (3), the power is 600 W, the gas pressure is 15 Torr, and the processing time is 4 min.
10. The high mobility n-type thin film of vertically assembled nano-diamond sheets as claimed in claim 1, characterized in that The high mobility n-type thin film assembled vertically from the nano-diamond sheets is prepared as follows: (1) Pretreatment of single crystal silicon substrate surface grinding and seeding: diamond powder and glycerol are fully dispersed and mixed to obtain diamond grinding paste; the diamond grinding paste is taken on a polishing flannel cloth, and an intrinsic single crystal silicon wafer is pressed back and forth on the grinding paste for 30 minutes. The polished silicon wafer is ultrasonically cleaned in acetone and anhydrous ethanol for 5 minutes in turn, and dried with nitrogen to obtain single crystal silicon after seeding; The volume of the glycerol is 100 mL / g based on the mass of the diamond powder; (2) Hot wire chemical vapor deposition thin film growth: the single crystal silicon after seeding described in step (1) is placed as a substrate in a hot wire chemical vapor deposition device, acetone is used as a carbon source, and the acetone is introduced into the reaction chamber by bubbling hydrogen with a flow rate of 90 sccm. At the same time, a flow rate of 200 sccm is introduced, and the growth power is controlled to be 2200 W and the growth pressure is 1.6 kPa to grow a nano-diamond particle layer for 20 minutes; the pure hydrogen flow rate is adjusted to 0 sccm and the hydrogen flow rate is 100 sccm, and the power is reduced to 1800 W to grow a vertical nano-diamond / graphene composite layer for 3 minutes; the introduction of pure hydrogen and acetone is stopped, and the power is slowly reduced to 0 at 0.5 V / min to obtain a silicon wafer containing a vertical nano-diamond / graphene composite layer; (3) Microwave argon / oxygen mixed plasma etching treatment: The silicon wafer containing the vertical nanodiamond / graphene composite sheet layer described in step (2) is placed in a microwave plasma vapor deposition device, and a mixed plasma of argon and oxygen is introduced, wherein the total flow rate of argon and oxygen is 100 sccm, and the flow rate of oxygen in the mixed plasma is controlled to be 10 sccm; the power is controlled to be 600 W, the gas pressure is 15 Torr, and the processing time is 4 min, to obtain a high-mobility n-type thin film with vertical assembly of the nanodiamond sheets.