Preparation and application of CuO / TiO2 catalyst for photocatalytic oxidation synthesis of benzaldehyde
By preparing CuO/TiO2 catalyst, the problems of harsh reaction conditions and environmental pollution in the traditional benzaldehyde synthesis process are solved, and the efficient synthesis of benzaldehyde at room temperature is achieved. The catalyst is cheap and environmentally friendly, with high conversion and selectivity.
Patent Information
- Application Number
- CN202310481035.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-04-28
AI Technical Summary
The traditional benzaldehyde synthesis process has problems such as harsh reaction conditions, inability to obtain both substrate conversion and selectivity, high production costs, and environmental pollution, and the visible light utilization rate of TiO2 materials is relatively low.
Using CuO/TiO2 catalyst, hydrothermal treatment was performed by adding TiO2 nanoparticles and sodium hydroxide solution to the polytetrafluoroethylene liner, followed by acidification and drying in an acidic environment, and then depositing CuO in ammonia water, and calcination was made 10 wt.% CuO/TiO2 catalyst, used for photocatalytic oxidation of benzaldehyde.
It realizes efficient and stable synthesis of benzaldehyde under normal temperature and pressure. The catalyst is cheap and easy to obtain, non-toxic and harmless, and can obtain high styrene conversion and benzaldehyde selectivity at the same time. The reaction conditions are mild and environmentally friendly.
Abstract
Description
Technical Field
[0001] The invention relates to the preparation and application of a CuO / TiO2 catalyst for synthesizing benzaldehyde through photocatalytic oxidation. Background Art
[0002] As the simplest aromatic aldehyde, benzaldehyde is widely used in pharmaceutical, perfume, agricultural chemical industry, food and other fields. The traditional processes for preparing benzaldehyde mainly include benzyl alcohol oxidation, toluene oxidation, benzoic acid hydrogenation reduction, toluene chlorination hydrolysis, etc. These synthesis processes have problems such as harsh reaction conditions, substrate conversion rate and benzaldehyde selectivity cannot be achieved at the same time, high production cost, and environmental pollution. For example, CN114700076A discloses a method for preparing a vanadium silver cerium composite metal oxide catalyst (V-Ag-Ce / TiO2) for preparing benzaldehyde by gas phase oxidation of toluene, with a molar ratio of V:Ag:Ce=4:2:1, a reaction temperature of 500°C, a catalyst dosage of 500 mg, a toluene conversion rate of 27.40%, and a benzaldehyde selectivity of 92.19%. Benzaldehyde can be synthesized by side chain oxidation of styrene. However, the traditional thermal catalytic oxidation of styrene to synthesize benzaldehyde also has problems such as harsh reaction conditions of high temperature or high pressure, high energy consumption, and the inability to achieve both styrene conversion rate and benzaldehyde selectivity.
[0003] The photocatalytic oxidation of styrene to synthesize benzaldehyde can be carried out at room temperature and pressure, with mild conditions, low energy consumption, and environmental friendliness. TiO2 materials are cheap, easy to obtain, efficient, stable, and environmentally friendly, so they are widely used in the field of photocatalysis. However, TiO2 has a large bandgap and low utilization rate of visible light. Therefore, TiO2 can be modified to enhance its catalytic effect under visible light. Summary of the invention
[0004] The purpose of the present invention is to provide a preparation and application of a CuO / TiO2 catalyst for synthesizing benzaldehyde by photocatalytic oxidation.
[0005] The present invention provides a method for preparing a CuO / TiO2 catalyst for photocatalytic oxidation synthesis of benzaldehyde, the conditions and steps are as follows: (1) preparing a carrier. 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1Acidify in hydrochloric acid solution for 12 h, and then wash with ultrapure water until neutral; finally, separate the solid product by centrifugation, dry and grind at 75 °C. The obtained sample is TiO2 carrier. (2) Prepare 10 wt.% CuO / TiO2 catalyst. Add 0.1000 g TiO2 carrier and 0.6~2.4 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 20-40℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-deposition; the obtained precipitate was washed with water until neutral, dried at 80°C for 12 h, and calcined in a muffle furnace at 180-500°C for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst.
[0006] The invention provides an application of a CuO / TiO2 catalyst for photocatalytic oxidation synthesis of benzaldehyde, and the conditions and steps are as follows: 50 mg of catalyst, 0.25-1 mL of styrene, 2.5-10 mL of acetonitrile and 1.5-6 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution are accurately added to a photocatalytic reactor, the reactor is sealed, and a xenon lamp (300 W, irradiation wavelength 400 nm) or natural light is used for irradiation under normal temperature circulating water cooling, and the reaction is stirred for 1-6 hours. After the reaction is completed, the catalyst solid and liquid are separated by centrifugation, the filtrate is analyzed by gas chromatography, and the conversion rate of styrene and the selectivity of benzaldehyde are calculated.
[0007] The beneficial effects of the present invention are as follows: the catalyst raw material is cheap, readily available, non-toxic, harmless, and stable in nature; the synthesis method is simple and easy; it is used in the photocatalytic oxidation reaction of styrene to synthesize benzaldehyde; the reaction conditions are mild, the environment is friendly, the reaction is efficient and stable, and a high styrene conversion rate and benzaldehyde selectivity can be obtained simultaneously.
[0008] Specific implementation method.
[0009] Example 1: 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 0.6 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 200℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.5 mL of styrene, 5 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, and the reactor was sealed. Under normal temperature circulating water cooling, a xenon lamp (300W, light wavelength 400 nm) was used for light irradiation and stirring for 3 h. After the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 25.6%, and the selectivity of benzaldehyde was 84.3%.
[0010] Example 2: 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 200℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.5 mL of styrene, 5 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, the reactor was sealed, and irradiated with a xenon lamp (300W, irradiation wavelength 400 nm) under normal temperature circulating water cooling, and stirred for 3 h; after the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 37.2%, and the selectivity of benzaldehyde was 82.3%.
[0011] Example 3: Add 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 2.4 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 200℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.5 mL of styrene, 5 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, and the reactor was sealed. Under normal temperature circulating water cooling, a xenon lamp (300W, light wavelength 400 nm) was used for light irradiation and stirring for 3 h. After the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 32.1%, and the selectivity of benzaldehyde was 82.7%.
[0012] Example 4: 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 20℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 200℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.5 mL of styrene, 5 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, the reactor was sealed, and irradiated with a xenon lamp (300W, light wavelength 400 nm) under normal temperature circulating water cooling, and stirred for 3 h; after the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 34.9%, and the selectivity of benzaldehyde was 80.7%.
[0013] Example 5: Add 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 40℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 200℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.5 mL of styrene, 5 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, and the reactor was sealed. Under normal temperature circulating water cooling, a xenon lamp (300W, light wavelength 400 nm) was used for light irradiation and stirring for 3 h. After the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 33.7%, and the selectivity of benzaldehyde was 77.5%.
[0014] Example 6: Add 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1ammonia water, ultrasonically treated for 10 min to make it evenly dispersed; then placed the beaker in a 30℃ water bath, stirred thoroughly for 1 h, 0.0420 g Cu(NO3)2·3H2O was dissolved in 4.2 mL ultrapure water, and slowly added to the above beaker, and continued stirring for 30 min. After the stirring, the obtained precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined in a muffle furnace at 200℃ for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. Into a photocatalytic reactor, 50 mg of catalyst, 0.5 mL of styrene, 5 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added, and the reactor was sealed. Under normal temperature circulating water cooling, the light source was irradiated with a xenon lamp (300 W, light wavelength 400 nm), and the reaction was stirred for 3 hours. After the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 23.7%, and the selectivity of benzaldehyde was 78.6%.
[0015] Example 7: Add 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was dried at 80°C for 12 h and then calcined at 200°C in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.5 mL of styrene, 5 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, the reactor was sealed, and the reaction was irradiated with a xenon lamp (300 W, irradiation wavelength 400 nm) under normal temperature circulating water cooling, and stirred for 3 h; after the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 28.6%, and the selectivity of benzaldehyde was 84.2%.
[0016] Example 8: Add 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 180℃ for 1 h in a muffle furnace to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.5 mL of styrene, 5 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, and the reactor was sealed. Under normal temperature circulating water cooling, a xenon lamp (300W, light wavelength 400 nm) was used for light irradiation and stirring for 3 h. After the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 27.9%, and the selectivity of benzaldehyde was 82.8%.
[0017] Example 9: Add 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 300℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.5 mL of styrene, 5 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, and the reactor was sealed. Under normal temperature circulating water cooling, a xenon lamp (300W, light wavelength 400 nm) was used for light irradiation and stirring for 3 h. After the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 30.1%, and the selectivity of benzaldehyde was 83.3%.
[0018] Example 10: Add 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 400℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.5 mL of styrene, 5 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, and the reactor was sealed. Under normal temperature circulating water cooling, a xenon lamp (300W, light wavelength 400 nm) was used for light irradiation and stirring for 3 h. After the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 30.8%, and the selectivity of benzaldehyde was 78.2%.
[0019] Example 11: Add 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 500℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.5 mL of styrene, 5 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, and the reactor was sealed. Under normal temperature circulating water cooling, a xenon lamp (300W, light wavelength 400 nm) was used for light irradiation and stirring for 3 h. After the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 19.5%, and the selectivity of benzaldehyde was 13.6%.
[0020] Example 12: Add 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 200℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.25 mL of styrene, 10 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, the reactor was sealed, and irradiated with a xenon lamp (300 W, irradiation wavelength 400 nm) under normal temperature circulating water cooling, and stirred for 6 h; after the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 67.8%, and the selectivity of benzaldehyde was 83.4%.
[0021] Example 13: Add 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The pH of the solution was adjusted to 9.5 by NaOH solution for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 200℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.5 mL of styrene, 10 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, and the reactor was sealed. Under normal temperature circulating water cooling, a xenon lamp (300W, light wavelength 400 nm) was used for light irradiation and stirring for 6 h. After the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 57.5%, and the selectivity of benzaldehyde was 82.6%.
[0022] Example 14: Add 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 200℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 1 mL of styrene, 10 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, and the reactor was sealed. Under normal temperature circulating water cooling, a xenon lamp (300W, light wavelength 400 nm) was used for light irradiation and stirring for 6 h. After the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 36.8%, and the selectivity of benzaldehyde was 81.3%.
[0023] Example 15: Add 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 200℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.25 mL of styrene, 2.5 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, the reactor was sealed, and irradiated with a xenon lamp (300 W, irradiation wavelength 400 nm) under normal temperature circulating water cooling, and stirred for 6 h; after the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 63.6%, and the selectivity of benzaldehyde was 80.2%.
[0024] Example 16: Add 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 200℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.25 mL of styrene, 5 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, the reactor was sealed, and irradiated with a xenon lamp (300W, irradiation wavelength 400 nm) under normal temperature circulating water cooling, and stirred for 6 h; after the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 52.4%, and the selectivity of benzaldehyde was 81.6%.
[0025] Example 17: Add 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 200℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.25 mL of styrene, 10 mL of acetonitrile and 1.5 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, the reactor was sealed, and the reaction was irradiated with a xenon lamp (300 W, irradiation wavelength 400 nm) under normal temperature circulating water cooling, and stirred for 6 h; after the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 41.6%, and the selectivity of benzaldehyde was 82.1%.
[0026] Example 18: Add 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 200℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.25 mL of styrene, 10 mL of acetonitrile and 6 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, the reactor was sealed, and irradiated with a xenon lamp (300 W, irradiation wavelength 400 nm) under normal temperature circulating water cooling, and stirred for 6 h; after the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 57.2%, and the selectivity of benzaldehyde was 79.6%.
[0027] Example 19: 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 200℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.25 mL of styrene, 10 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, the reactor was sealed, and irradiated with a xenon lamp (300 W, irradiation wavelength 400 nm) under normal temperature circulating water cooling, and stirred for 1 h; after the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 11.5%, and the selectivity of benzaldehyde was 94.0%.
[0028] Example 20: 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 200℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.25 mL of styrene, 10 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, the reactor was sealed, and the reaction was irradiated with a xenon lamp (300 W, irradiation wavelength 400 nm) under normal temperature circulating water cooling, and stirred for 3 h; after the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 38.6%, and the selectivity of benzaldehyde was 86.3%.
[0029] Example 21: Add 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 °C. The obtained sample was TiO2 carrier. 0.1000 g TiO2 carrier and 1.2 mL 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80°C for 12 h, and calcined at 200°C in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.25 mL of styrene, 10 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, the reactor was sealed, and under normal temperature circulating water cooling, natural light was used for irradiation and stirring for 6 h; after the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 66.9%, and the selectivity of benzaldehyde was 83.2%.
[0030] Example 22: 0.25 mL of styrene, 10 mL of acetonitrile and 3 mL of 70 wt.% aqueous tert-butyl hydroperoxide solution were accurately added to a photocatalytic reactor, the reactor was sealed, and irradiated with a xenon lamp (300 W, light wavelength 400 nm) under normal temperature circulating water cooling, and the reaction was stirred for 6 h. After the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 1.4%, and the selectivity of benzaldehyde was 17.8%.
[0031] Example 23: 1.0000 g of anatase TiO2 nanoparticles and 50 mL of 10 mol·L -1Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed; the liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral; then 250 mL 0.1 mol·L -1 Acidification in hydrochloric acid solution for 12 h, and then washed with ultrapure water until neutral; finally, the solid product was separated by centrifugation, dried and ground at 75 ° C, and the obtained sample was TiO2 carrier. 50 mg TiO2 carrier, 0.25 mL styrene, 10 mL acetonitrile and 3 mL 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, and the reactor was sealed. Under normal temperature circulating water cooling, a xenon lamp (300 W, light wavelength 400 nm) was used for light irradiation and stirring for 6 h; after the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 17.9%, and the selectivity of benzaldehyde was 3.1%.
[0032] Example 24: 0.1000 g of anatase TiO2 nanoparticles and 1.2 mL of 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed; then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-precipitation; the precipitate was washed with water until neutral, dried at 80℃ for 12 h, and calcined at 200℃ in a muffle furnace for 1 h to obtain a 10 wt.% CuO / TiO2 catalyst. 50 mg of catalyst, 0.25 mL of styrene, 10 mL of acetonitrile and 3 mL of 70 wt.% tert-butyl hydroperoxide aqueous solution were accurately added to the photocatalytic reactor, the reactor was sealed, and irradiated with a xenon lamp (300 W, irradiation wavelength 400 nm) under normal temperature circulating water cooling, and stirred for 6 h; after the reaction, the catalyst solid and liquid were separated by centrifugation, and the filtrate was analyzed by gas chromatography. The conversion rate of styrene was 22.6%, and the selectivity of benzaldehyde was 74.8%.
Claims
1. An application of a CuO / TiO2 catalyst for photocatalytic oxidation synthesis of benzaldehyde, characterized in that: Accurately add 50mg CuO / TiO2 catalyst, 0.25mL styrene, 10mL acetonitrile and 3mL 70wt.% tert-butyl hydroperoxide aqueous solution into a photocatalytic reactor, seal the reactor, and irradiate with xenon lamp light source or natural light under normal temperature circulating water cooling, stir and react for 6h. After the reaction, centrifuge to separate the catalyst solid and liquid, and analyze the liquid by gas chromatography. The parameters of the xenon lamp light source are 300W power and 400nm light wavelength. Under the conditions, the conversion rate of styrene is 67.8% and the selectivity of benzaldehyde is 83.4%. Under the natural light condition, the conversion rate of styrene is 66.9% and the selectivity of benzaldehyde is 83.2%. The preparation method of the CuO / TiO2 catalyst is as follows: 1.0000g anatase TiO2 nanoparticles and 50mL 10mol·L -1 Sodium hydroxide solution was stirred vigorously for 30 min and then ultrasonically treated for 30 min to make it evenly dispersed. The liner was sealed in a hydrothermal reactor and hydrothermally treated at 130 °C for 48 h. After the temperature dropped to room temperature, the solid was washed with ultrapure water until neutral, and then in 250 mL 0.1 mol·L -1 The product was acidified in a hydrochloric acid solution for 12 h, washed again with ultrapure water until neutral, and finally centrifuged to separate the solid product, which was dried and ground at 75 °C. The obtained sample was a TiO2 carrier. 0.1000 g of TiO2 carrier and 1.2 mL of 0.3 mol·L -1 ammonia water, ultrasonically treat for 10 min to make it evenly dispersed, then place the beaker in a 30℃ water bath, stir thoroughly for 1 h, dissolve 0.0420 g Cu(NO3)2·3H2O in 4.2 mL ultrapure water, and slowly drop it into the beaker, continue stirring for 30 min, and then add 1 mol·L -1 The NaOH solution was adjusted to pH 9.5 for co-deposition, the obtained precipitate was washed with water until neutral, dried at 80° C. for 12 h, and calcined in a muffle furnace at 200° C. for 1 h to obtain the CuO / TiO2 catalyst.