A black photovoltaic interconnection welding rod and a preparation method thereof
By setting up conductive copper-based and tin nickel copper-bismuth alloy hollow welding layers on the photovoltaic interconnection strip, the problem of blackening and welding of small-sized photovoltaic interconnection strips is solved, and the efficient blackening and welding effect is achieved, which improves the appearance of photovoltaic components Aesthetics and welding reliability.
Patent Information
- Application Number
- CN202310351694.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-04-04
AI Technical Summary
The prior art is difficult to achieve blackening and efficient welding on small-sized photovoltaic interconnect strips, and the existing black coating lacks conductivity, resulting in frequent false welding problems.
A black photovoltaic interconnection electrode consisting of a conductive copper base, a first welding layer and a second black micro hollow welding layer is a tin nickel copper bismuth alloy layer, and the conductive copper base tin plating, corrosion treatment and The process of electroplating the tin nickel copper-bismuth alloy layer forms a black plating layer with low temperature melting characteristics.
The blackening of small-size photovoltaic interconnection strips and the full blackening of the entire photovoltaic module are achieved, which improves the reliability and appearance of welding and ensures the reliability of the solder joints.
Smart Images

Figure CN116475619B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of photovoltaic materials, and more specifically, to a black photovoltaic interconnection welding rod and a preparation method thereof. Background Art
[0002] Black photovoltaic modules are simple and elegant in color and have always been popular in Europe and the United States. At present, the black modules exported by domestic module manufacturers cannot be called all-black modules in the strict sense. The photovoltaic interconnection strips connecting the solar cells are still mainly made of silver-white tin-lead alloy because they need to be welded.
[0003] Patent number CN112397606A proposes to use a method of spraying a black coating to achieve the blackening of photovoltaic interconnection strips, but this method has many disadvantages. First, photovoltaic interconnection strips are smaller in size than photovoltaic bus bars, and it is very difficult to implement a segmented spraying process on a smaller size; secondly, photovoltaic interconnection strips are currently mainly circular or triangular, and single-sided printing cannot be achieved; most importantly, the black coating itself has no conductive effect and cannot form a complete circuit with the silicon cell. After spraying it on the surface of the photovoltaic interconnection strip, welding cannot be achieved, or it is easy to cause cold welding.
[0004] Patent number CN113178502A proposes to use laser etching to form an etching layer and achieve a black effect through multiple diffuse reflections of light. This process can only form a black effect on a single-side regular surface, but not on circular photovoltaic interconnection strips. Moreover, for circular photovoltaic interconnection strips, the winding and unwinding process cannot identify the welding surface and the non-welding surface, and it is easy to cause the welding surface and the non-welding surface to be inverted, resulting in cold soldering or color difference problems.
[0005] Patent number CN205443483U proposes a highly solderable tin-nickel alloy coating. The melting point of the electroplated layer alloy is relatively high. Increasing the welding temperature can easily cause hidden cracks in the battery cell. It has no hollow structure. Secondly, the outer solder is wrapped by the outer alloy layer and cannot overflow quickly. It is easy to cause cold solder joints when used in the photovoltaic industry.
[0006] Therefore, a new solution needs to be proposed to solve this problem. Summary of the invention
[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a black photovoltaic interconnection welding rod and a preparation method thereof. By setting two welding layers, it can not only solve the welding problem of the black photovoltaic interconnection strip, but also realize the blackening of the photovoltaic interconnection strip.
[0008] The above technical purpose of the present invention is achieved through the following technical scheme: a black photovoltaic interconnection welding rod, comprising a conductive copper base, a first welding layer and a second black microscopic hollow welding layer arranged in sequence from the inside to the outside, and the second black microscopic hollow welding layer is a tin-nickel-copper-bismuth alloy layer.
[0009] In one embodiment, the thickness of the first soldering layer is 10um-25um, and the first soldering layer is a lead-containing low-temperature tin layer or a lead-free low-temperature tin layer.
[0010] In one embodiment, the thickness of the second black microscopic hollow welding layer is 0.5um-1um, and the second black microscopic hollow welding layer comprises an alloy having the following mass ratio:
[0011] Nickel 30%-35%, bismuth 5%-15%, copper 0.05%-5%, and the rest are tin and inevitable impurities.
[0012] A method for preparing a black photovoltaic interconnection welding rod comprises any of the above-mentioned black photovoltaic interconnection welding rods, and further comprises the following steps:
[0013] S1. Tin plating of conductive copper base: After the conductive copper base is treated with a flux treatment liquid, a lead-containing low-temperature tin or a lead-free low-temperature tin is coated on the conductive copper base by immersion plating to form a lead-containing low-temperature tin layer or a lead-free low-temperature tin layer on the conductive copper base, and after cooling, the conductive copper base is rolled up;
[0014] S2. Corrosion treatment is performed on the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer: a weak acid is used to slightly corrode the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer, so that dense microscopic hollow pits are formed on the surface, and then a multi-pass ultrasonic cleaning process is quickly used to clean the residual weak acid on the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer to obtain a semi-finished product;
[0015] S3. Electroplating of tin-nickel-copper-bismuth alloy layer: Add tin-nickel-copper-bismuth electroplating solution into the electroplating tank, and set the current density of the electroplating tank to 1A / dm 2 -2A / dm 2 , the temperature of the tin-nickel-copper-bismuth electroplating solution is set to 30° C.-50° C., the semi-finished product obtained in step S2 is immersed in the tin-nickel-copper-bismuth electroplating solution, and ultrasonic assistance is intermittently added. After 1 min.-3 min., the second black microscopic hollow welding layer is formed on the surface of the semi-finished product, thereby obtaining the black photovoltaic interconnection welding rod;
[0016] The formula components and contents of the tin-nickel-copper-bismuth electroplating solution are as follows: 10 g / L-20 g / L stannous sulfate, 5 g / L-20 g / L bismuth sulfate, 10 g / L-20 g / L nickel sulfate, 0.3 g / L-2 g / L copper sulfate, 100 g / L-300 g / L potassium pyrophosphate, 0.5 g / L-5 g / L pore-forming auxiliary agent, and 2 g / L-6 g / L blackening agent.
[0017] In one embodiment, the pore-forming auxiliary agent is at least one of an amine substance, a quaternary ammonium salt substance, and a sodium carboxylate salt.
[0018] In one embodiment, the blackening agent is at least one of the nitrogen-containing amino acids mercaptoalanine, homocysteine, and sulfur-containing amino acids.
[0019] In summary, the present invention has the following beneficial effects:
[0020] 1. The present invention realizes the blackening of small-sized photovoltaic interconnection strips and the full blackening of the entire photovoltaic module by setting a double welding layer structure of a first welding layer and a second black microscopic hollow welding layer, making the appearance of the photovoltaic module more exquisite;
[0021] 2. In the present invention, the second black microscopic hollow welding layer adopts a tin-nickel-copper-bismuth alloy layer. The tin-nickel-copper-bismuth alloy has the characteristic of melting at low temperature, thereby solving the low-temperature weldability of the black coating;
[0022] 3. The present invention combines a pore-forming auxiliary agent with an ultrasonic process to make the microscopic hollow pores of the second black microscopic hollow welding layer more uniform, thereby ensuring the weldability of each welding point of the interconnected welding rod. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A schematic diagram of the structure of a black photovoltaic interconnection welding rod according to an embodiment of the present application;
[0024] Figure 2 This is a flowchart of a method for preparing a black photovoltaic interconnect welding rod according to an embodiment of the present application.
[0025] In the figure: 1. Conductive copper base; 2. First welding layer; 3. Second black micro-hollow welding layer. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] like Figure 1 and Figure 2 As shown, an embodiment of the present application provides a black photovoltaic interconnect welding rod, comprising a conductive copper base 1, a first welding layer 2 and a second black microscopic hollow welding layer 3 arranged in sequence from the inside to the outside, wherein the second black microscopic hollow welding layer 3 is a tin-nickel-copper-bismuth alloy layer.
[0028] In the above-mentioned black photovoltaic interconnection welding rod, the first welding layer 2 plays the actual welding role, and the second black microscopic hollow welding layer 3 plays the role of auxiliary welding and black appearance. Through the setting of the first welding layer 2 and the second black microscopic hollow welding layer 3, it is possible to solve the welding problem of the black photovoltaic interconnection strip and realize the blackening of the photovoltaic interconnection strip. Among them, the second black microscopic hollow welding layer 3 adopts a tin-nickel-copper-bismuth alloy layer. The tin-nickel-copper-bismuth alloy has the characteristic of low-temperature melting, thereby solving the low-temperature weldability of the black coating.
[0029] In this embodiment, the thickness of the first soldering layer 2 is 10um-25um, and the first soldering layer 2 is a lead-containing low-temperature tin layer or a lead-free low-temperature tin layer.
[0030] By setting the thickness of the first welding layer 2 to 10um-25um, sufficient tin in the first welding layer that actually performs welding can flow out from the micropores of the second black microscopic hollow welding layer 3 to form welding points, thus avoiding the problem of cold soldering.
[0031] In this embodiment, the thickness of the second black microscopic hollow welding layer 3 is 0.5um-1um, and the second black microscopic hollow welding layer 3 includes the following alloys in mass ratio:
[0032] Nickel 30%-35%, bismuth 5%-15%, copper 0.05%-5%, and the rest are tin and inevitable impurities.
[0033] The specific mass ratio of nickel can be 30%, 31%, 32%, 33%, 34%, and 35%, the mass ratio of bismuth can be 5%, 10%, and 15%, and the mass ratio of copper can be 0.05, 0.1%, 1%, 2%, 3%, 4%, and 5%. The optimal option is that the mass ratio of nickel is 32%, the mass ratio of bismuth can be 5%, and the mass ratio of copper can be 2%. In this way, the second black microscopic hollow welding layer 3 has the advantages of good blackening and hollowing effects.
[0034] In the above setting, if the thickness of the second black microscopic hollow welding layer is too thin, its color will be interfered by the silver color of the first welding layer, resulting in the black color not being obvious. If the thickness of the second black microscopic hollow welding layer is too thick, its micropores will be enlarged, which will easily mix with the silver color to form mixed colors, resulting in poor appearance and not conducive to the outflow of tin. Therefore, within the thickness range of the above-mentioned second black microscopic hollow welding layer 3, the effect of the black photovoltaic interconnection welding rod in this embodiment can reach the best state.
[0035] The present application also provides a method for preparing a black photovoltaic interconnect welding rod according to the following embodiment:
[0036] Embodiment 1:
[0037] A method for preparing a black photovoltaic interconnection welding rod comprises any of the above-mentioned black photovoltaic interconnection welding rods, and further comprises the following steps:
[0038] S1, tinning the conductive copper base 1: after the conductive copper base 1 is treated with a flux treatment liquid, a lead-containing low-temperature tin or a lead-free low-temperature tin is coated on the conductive copper base 1 by immersion plating to form a lead-containing low-temperature tin layer or a lead-free low-temperature tin layer on the conductive copper base 1, and after cooling, the conductive copper base 1 is rolled up;
[0039] S2. Corrosion treatment is performed on the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer: a weak acid is used to slightly corrode the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer, so that dense microscopic hollow pits are formed on the surface, and then a multi-pass ultrasonic cleaning process is quickly used to clean the residual weak acid on the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer to obtain a semi-finished product;
[0040] S3, electroplating a tin-nickel-copper-bismuth alloy layer: adding a tin-nickel-copper-bismuth electroplating solution into an electroplating tank, setting the current density of the electroplating tank to 1.4 A / dm2, setting the temperature of the tin-nickel-copper-bismuth electroplating solution to 45°C, immersing the semi-finished product obtained in step S2 into the tin-nickel-copper-bismuth electroplating solution, and controlling the ultrasonic device to intermittently add ultrasonic assistance through the control module, so that the bubbles generated on the surface of the tin-nickel-copper-bismuth alloy layer can disappear regularly. After 1.6 minutes, the second black microscopic hollow welding layer 3 with a thickness of about 0.6 um is formed on the surface of the semi-finished product, thereby obtaining the black photovoltaic interconnection welding rod;
[0041] The formula components and contents of the tin-nickel-copper-bismuth electroplating solution are as follows: 14 g / L stannous sulfate, 6 g / L bismuth sulfate, 10 g / L nickel sulfate, 0.5 g / L copper sulfate, 200 g / L potassium pyrophosphate, 0.5 g / L-5 g / L pore-forming auxiliary agent and 2.5 g / L blackening agent.
[0042] Specifically, the pore-forming auxiliary agent is at least one of an amine substance, a quaternary ammonium salt substance, and a sodium carboxylate salt. In this embodiment, the preferred pore-forming auxiliary agent includes 0.3 g / L sodium acetate and 0.3 g / L triethylamine.
[0043] Specifically, the blackening agent is at least one of nitrogen-containing amino acids mercaptoalanine, homocysteine, and sulfur-containing amino acids. In this embodiment, the preferred blackening agent is methionine.
[0044] Through the above settings, the surface coating of the interconnection bar is bright black, and when soldered at 200°C, the tin layer can overflow evenly and the soldering points are firm.
[0045] Embodiment 2:
[0046] A method for preparing a black photovoltaic interconnection welding rod comprises any of the above-mentioned black photovoltaic interconnection welding rods, and further comprises the following steps:
[0047] S1, tinning the conductive copper base 1: after the conductive copper base 1 is treated with a flux treatment liquid, a lead-containing low-temperature tin or a lead-free low-temperature tin is coated on the conductive copper base 1 by immersion plating to form a lead-containing low-temperature tin layer or a lead-free low-temperature tin layer on the conductive copper base 1, and after cooling, the conductive copper base 1 is rolled up;
[0048] S2. Corrosion treatment is performed on the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer: a weak acid is used to slightly corrode the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer, so that dense microscopic hollow pits are formed on the surface, and then a multi-pass ultrasonic cleaning process is quickly used to clean the residual weak acid on the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer to obtain a semi-finished product;
[0049] S3, electroplating a tin-nickel-copper-bismuth alloy layer: adding a tin-nickel-copper-bismuth electroplating solution into an electroplating tank, setting the current density of the electroplating tank to 1.5 A / dm2, setting the temperature of the tin-nickel-copper-bismuth electroplating solution to 43°C, immersing the semi-finished product obtained in step S2 into the tin-nickel-copper-bismuth electroplating solution, intermittently adding ultrasonic assistance, and after 2.0 minutes, forming the second black microscopic hollow welding layer 3 with a thickness of about 0.7 um on the surface of the semi-finished product, thereby obtaining the black photovoltaic interconnection welding rod;
[0050] Among them, the formula components and contents of the tin-nickel-copper-bismuth electroplating solution are: 16 g / L stannous sulfate, 7 g / L bismuth sulfate, 10.5 g / L nickel sulfate, 0.7 g / L copper sulfate, 220 g / L potassium pyrophosphate, 0.5 g / L-5 g / L pore-forming auxiliary agent and 2.5 g / L blackening agent.
[0051] Specifically, the pore-forming auxiliary agent is at least one of an amine substance, a quaternary ammonium salt substance, and a sodium carboxylate salt. In this embodiment, the preferred pore-forming auxiliary agent includes 0.2 g / L sodium acetate and 0.4 g / L triethylamine.
[0052] Specifically, the blackening agent is at least one of nitrogen-containing amino acids mercaptoalanine, homocysteine, and sulfur-containing amino acids. In this embodiment, the preferred blackening agent is methionine.
[0053] Through the above settings, the surface coating of the interconnection bar is bright black, and when soldered at 196°C, the tin layer can overflow evenly and the soldering points are firm.
[0054] Embodiment 3:
[0055] A method for preparing a black photovoltaic interconnection welding rod comprises any of the above-mentioned black photovoltaic interconnection welding rods, and further comprises the following steps:
[0056] S1, tinning the conductive copper base 1: after the conductive copper base 1 is treated with a flux treatment liquid, a lead-containing low-temperature tin or a lead-free low-temperature tin is coated on the conductive copper base 1 by immersion plating to form a lead-containing low-temperature tin layer or a lead-free low-temperature tin layer on the conductive copper base 1, and after cooling, the conductive copper base 1 is rolled up;
[0057] S2. Corrosion treatment is performed on the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer: a weak acid is used to slightly corrode the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer, so that dense microscopic hollow pits are formed on the surface, and then a multi-pass ultrasonic cleaning process is quickly used to clean the residual weak acid on the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer to obtain a semi-finished product;
[0058] S3, electroplating a tin-nickel-copper-bismuth alloy layer: adding a tin-nickel-copper-bismuth electroplating solution into an electroplating tank, setting the current density of the electroplating tank to 1.5 A / dm2, setting the temperature of the tin-nickel-copper-bismuth electroplating solution to 40°C, immersing the semi-finished product obtained in step S2 into the tin-nickel-copper-bismuth electroplating solution, intermittently adding ultrasonic assistance, and after 2.5 minutes, forming the second black microscopic hollow welding layer 3 with a thickness of about 0.8 um on the surface of the semi-finished product, thereby obtaining the black photovoltaic interconnect welding rod;
[0059] Among them, the formula components and contents of the tin-nickel-copper-bismuth electroplating solution are: 18 g / L stannous sulfate, 8 g / L bismuth sulfate, 10 g / L nickel sulfate, 0.6 g / L copper sulfate, 230 g / L potassium pyrophosphate, 0.5 g / L-5 g / L pore-forming auxiliary agent and 2.5 g / L blackening agent.
[0060] Specifically, the pore-forming auxiliary agent is at least one of an amine substance, a quaternary ammonium salt substance, and a sodium carboxylate salt. In this embodiment, the preferred pore-forming auxiliary agent includes 0.3 g / L sodium acetate and 0.5 g / L triethylamine.
[0061] Specifically, the blackening agent is at least one of nitrogen-containing amino acids mercaptoalanine, homocysteine, and sulfur-containing amino acids. In this embodiment, the preferred blackening agent is methionine.
[0062] Through the above settings, the surface coating of the interconnection bar is bright black, and when soldered at 194°C, the tin layer can overflow evenly and the soldering points are firm.
[0063] Embodiment 4:
[0064] A method for preparing a black photovoltaic interconnection welding rod comprises any of the above-mentioned black photovoltaic interconnection welding rods, and further comprises the following steps:
[0065] S1, tinning the conductive copper base 1: after the conductive copper base 1 is treated with a flux treatment liquid, a lead-containing low-temperature tin or a lead-free low-temperature tin is coated on the conductive copper base 1 by immersion plating to form a lead-containing low-temperature tin layer or a lead-free low-temperature tin layer on the conductive copper base 1, and after cooling, the conductive copper base 1 is rolled up;
[0066] S2. Corrosion treatment is performed on the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer: a weak acid is used to slightly corrode the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer, so that dense microscopic hollow pits are formed on the surface, and then a multi-pass ultrasonic cleaning process is quickly used to clean the residual weak acid on the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer to obtain a semi-finished product;
[0067] S3, electroplating a tin-nickel-copper-bismuth alloy layer: adding a tin-nickel-copper-bismuth electroplating solution into an electroplating tank, setting the current density of the electroplating tank to 1.6 A / dm2, setting the temperature of the tin-nickel-copper-bismuth electroplating solution to 43°C, immersing the semi-finished product obtained in step S2 into the tin-nickel-copper-bismuth electroplating solution, intermittently adding ultrasonic assistance, and after 3.0 minutes, forming the second black microscopic hollow welding layer 3 with a thickness of about 1.0 um on the surface of the semi-finished product, thereby obtaining the black photovoltaic interconnection welding rod;
[0068] Among them, the formula components and contents of the tin-nickel-copper-bismuth electroplating solution are: 20g / L stannous sulfate, 9g / L bismuth sulfate, 10g / L nickel sulfate, 0.6g / L copper sulfate, 220g / L potassium pyrophosphate, 0.5g / L-5g / L pore-forming auxiliary agent and 2.5g / L blackening agent.
[0069] Specifically, the pore-forming auxiliary agent is at least one of an amine substance, a quaternary ammonium salt substance, and a sodium carboxylate salt. In this embodiment, the preferred pore-forming auxiliary agent includes 0.4 g / L sodium acetate and 0.2 g / L triethylamine.
[0070] Specifically, the blackening agent is at least one of nitrogen-containing amino acids mercaptoalanine, homocysteine, and sulfur-containing amino acids. In this embodiment, the preferred blackening agent is methionine.
[0071] Through the above settings, the surface coating of the interconnection bar is bright black, and when soldered at 190°C, the tin layer can overflow evenly and the soldering points are firm.
[0072] Comparative Example 1:
[0073] A method for preparing a black photovoltaic interconnection welding rod comprises any of the above-mentioned black photovoltaic interconnection welding rods, and further comprises the following steps:
[0074] S1, tinning the conductive copper base 1: after the conductive copper base 1 is treated with a flux treatment liquid, a lead-containing low-temperature tin or a lead-free low-temperature tin is coated on the conductive copper base 1 by immersion plating to form a lead-containing low-temperature tin layer or a lead-free low-temperature tin layer on the conductive copper base 1, and after cooling, the conductive copper base 1 is rolled up;
[0075] S2. Corrosion treatment is performed on the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer: a weak acid is used to slightly corrode the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer, so that dense microscopic hollow pits are formed on the surface, and then a multi-pass ultrasonic cleaning process is quickly used to clean the residual weak acid on the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer to obtain a semi-finished product;
[0076] S3, electroplating a tin-nickel-copper-bismuth alloy layer: adding a tin-nickel-copper-bismuth electroplating solution into an electroplating tank, setting the current density of the electroplating tank to 1.5 A / dm2, setting the temperature of the tin-nickel-copper-bismuth electroplating solution to 43°C, immersing the semi-finished product obtained in step S2 into the tin-nickel-copper-bismuth electroplating solution, intermittently adding ultrasonic assistance, and after 2.0 minutes, forming the second black microscopic hollow welding layer 3 with a thickness of about 0.7 um on the surface of the semi-finished product, thereby obtaining the black photovoltaic interconnection welding rod;
[0077] The formula components and contents of the tin-nickel-copper-bismuth electroplating solution are as follows: 16 g / L stannous sulfate, 7 g / L bismuth sulfate, 10.5 g / L nickel sulfate, 0.7 g / L copper sulfate, 220 g / L potassium pyrophosphate, 0.4 g / L sodium hydroxide and 2.5 g / L blackening agent.
[0078] Specifically, the blackening agent is at least one of nitrogen-containing amino acids mercaptoalanine, homocysteine, and sulfur-containing amino acids. In this embodiment, the preferred blackening agent is methionine.
[0079] Through the above settings, the surface coating of the interconnection bar is bright black, and when soldered at 240°C, the tin layer is difficult to overflow and the solder joint cold soldering rate is high.
[0080] Comparative Example 2:
[0081] A method for preparing a black photovoltaic interconnection welding rod comprises any of the above-mentioned black photovoltaic interconnection welding rods, and further comprises the following steps:
[0082] S1, tinning the conductive copper base 1: after the conductive copper base 1 is treated with a flux treatment liquid, a lead-containing low-temperature tin or a lead-free low-temperature tin is coated on the conductive copper base 1 by immersion plating to form a lead-containing low-temperature tin layer or a lead-free low-temperature tin layer on the conductive copper base 1, and after cooling, the conductive copper base 1 is rolled up;
[0083] S2. Corrosion treatment is performed on the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer: a weak acid is used to slightly corrode the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer, so that dense microscopic hollow pits are formed on the surface, and then a multi-pass ultrasonic cleaning process is quickly used to clean the residual weak acid on the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer to obtain a semi-finished product;
[0084] S3, electroplating a tin-nickel-copper-bismuth alloy layer: adding a tin-nickel-copper-bismuth electroplating solution into an electroplating tank, setting the current density of the electroplating tank to 1.5 A / dm2, and setting the temperature of the tin-nickel-copper-bismuth electroplating solution to 43°C, immersing the semi-finished product obtained in step S2 into the tin-nickel-copper-bismuth electroplating solution, and after 2.0 minutes, forming the second black microscopic hollow welding layer 3 with a thickness of about 0.7 um on the surface of the semi-finished product, thereby obtaining the black photovoltaic interconnect welding rod;
[0085] Among them, the formula components and contents of the tin-nickel-copper-bismuth electroplating solution are: 18 g / L stannous sulfate, 8 g / L bismuth sulfate, 10 g / L nickel sulfate, 0.6 g / L copper sulfate, 230 g / L potassium pyrophosphate, 0.5 g / L-5 g / L pore-forming auxiliary agent and 2.5 g / L blackening agent.
[0086] Specifically, the pore-forming auxiliary agent is at least one of an amine substance, a quaternary ammonium salt substance, and a sodium carboxylate salt. In this embodiment, the preferred pore-forming auxiliary agent includes 0.3 g / L sodium acetate and 0.5 g / L triethylamine.
[0087] Specifically, the blackening agent is at least one of nitrogen-containing amino acids mercaptoalanine, homocysteine, and sulfur-containing amino acids. In this embodiment, the preferred blackening agent is methionine.
[0088] Through the above settings, the surface coating of the interconnection bar is bright black, and when soldered at 260°C, the tin layer is difficult to overflow and the solder joint cold soldering rate is high.
[0089] From the comparison of Examples 1-4, it is found that as the stannous sulfate content in the tin-nickel-copper-bismuth electroplating solution increases, the stannous sulfate content in the tin-nickel-copper-bismuth alloy layer also increases accordingly. At this time, the welding temperature can be appropriately adjusted down. Since the black effect of the tin-nickel-copper-bismuth alloy layer is mainly determined by nickel sulfate, when the stannous sulfate content increases, the nickel sulfate content with the same color effect will be relatively reduced. Therefore, it is necessary to appropriately increase the thickness of the tin-nickel-copper-bismuth alloy layer to achieve the same color effect.
[0090] By comparing Example 2 with Comparative Example 1, it is found that when no pore-forming auxiliary agent is added, the tin-nickel-copper-bismuth alloy layer has only scattered hollow points. During welding, the tin layer is difficult to overflow, resulting in poor welding.
[0091] By comparing Example 2 and Comparative Example 2, it is found that when intermittent ultrasonic assistance is not added, scattered and large pits will appear on the surface of the tin-nickel-copper-bismuth alloy layer. This is because when the tin-nickel-copper-bismuth alloy layer is electroplated, the bubbles generated on its surface are not eliminated in time and remain attached to the same place, resulting in the inability to evenly plate the alloy layer around it.
[0092] In summary, the present invention realizes the blackening of small-sized photovoltaic interconnection strips and the full blackening of the entire photovoltaic module through the setting of a double welding layer structure of a first welding layer 2 and a second black microscopic hollow welding layer 3, making the appearance of the photovoltaic module more exquisite; the second black microscopic hollow welding layer 3 adopts a tin-nickel-copper-bismuth alloy layer, and the tin-nickel-copper-bismuth alloy has the characteristic of low-temperature melting, thereby solving the low-temperature weldability of the black coating; through the combination of a pore-forming auxiliary agent and an ultrasonic process, the microscopic hollow pores of the second black microscopic hollow welding layer 3 are made more uniform, thereby ensuring the weldability of each welding point of the interconnection welding rod.
[0093] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A black photovoltaic interconnection welding rod, characterized in that: It includes a conductive copper base, a first welding layer, and a second black microscopic hollow welding layer arranged in sequence from the inside to the outside, wherein the second black microscopic hollow welding layer is a tin-nickel-copper-bismuth alloy layer; The thickness of the second black microscopic hollow welding layer is 0.5um-1um, and the second black microscopic hollow welding layer comprises the following alloys in mass ratio: Nickel 30%-35%, bismuth 5%-15%, copper 0.05%-5%, and the rest are tin and inevitable impurities.
2. The black photovoltaic interconnection welding rod according to claim 1, characterized in that: The thickness of the first soldering layer is 10um-25um, and the first soldering layer is a lead-containing low-temperature tin layer or a lead-free low-temperature tin layer.
3. A method for preparing a black photovoltaic interconnection welding rod, characterized in that: The method comprises the black photovoltaic interconnection welding rod as claimed in any one of claims 1 to 2, and further comprises the following steps: S1. Tin plating of conductive copper base: After the conductive copper base is treated with a flux treatment liquid, a lead-containing low-temperature tin or a lead-free low-temperature tin is coated on the conductive copper base by immersion plating to form a lead-containing low-temperature tin layer or a lead-free low-temperature tin layer on the conductive copper base, and after cooling, the conductive copper base is rolled up; S2. Corrosion treatment is performed on the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer: a weak acid is used to slightly corrode the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer, so that dense microscopic hollow pits are formed on the surface, and then a multi-pass ultrasonic cleaning process is quickly used to clean the residual weak acid on the surface of the lead-containing low-temperature tin layer or the lead-free low-temperature tin layer to obtain a semi-finished product; S3. Electroplating of tin-nickel-copper-bismuth alloy layer: Add tin-nickel-copper-bismuth electroplating solution into the electroplating tank, and set the current density of the electroplating tank to 1A / dm 2 -2A / dm 2 , the temperature of the tin-nickel-copper-bismuth electroplating solution is set to 30° C.-50° C., the semi-finished product obtained in step S2 is immersed in the tin-nickel-copper-bismuth electroplating solution, and ultrasonic assistance is intermittently added. After 1 min.-3 min., the second black microscopic hollow welding layer is formed on the surface of the semi-finished product, thereby obtaining the black photovoltaic interconnection welding rod; Among them, the formula components and contents of the tin-nickel-copper-bismuth electroplating solution are: stannous sulfate 10g / L-20g / L, bismuth sulfate 5g / L-20g / L, nickel sulfate 10g / L-20g / L, copper sulfate 0.3g / L-2g / L, potassium pyrophosphate 100g / L-300g / L, pore-forming auxiliary agent 0.5g / L-5g / L and blackening agent 2g / L-6g / L.
4. The method for preparing a black photovoltaic interconnection welding rod according to claim 3, characterized in that: The pore-forming auxiliary agent is at least one of an amine substance, a quaternary ammonium salt substance, and a sodium carboxylate salt.
5. The method for preparing a black photovoltaic interconnection welding rod according to claim 3, characterized in that: The blackening agent is at least one of nitrogen-containing amino acids mercaptoalanine, homocysteine, and sulfur-containing amino acids.