Silver nanoconductive filler that can overcome the coffee ring effect

By reacting a coating agent with ethylene glycol and inorganic salts in silver nano conductive ink, a silver nano conductive filler that can overcome the coffee ring effect is prepared, and water is used as a solvent to achieve low-temperature drying and solve the problems in the existing technology. coffee ring effect and high temperature problems, an efficient, low-cost and environmentally friendly conductive ink was obtained.

CN116478576BActive Publication Date: 2024-10-01TIANJIN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210037923.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-13
Publication Date
2024-10-01
Estimated Expiration
2042-01-13

AI Technical Summary

Technical Problem

Existing silver nanoconductive inks often suffer from the coffee ring effect during the printing process, causing the middle part of the printed pattern to be non-conductive and the edges to be rough. Moreover, traditional methods use harmful solvents and high-temperature drying, making it difficult to achieve a low-cost and environmentally friendly solution. plan.

Method used

Mix the coating agent with ethylene glycol, heat it to 100-200°C, add inorganic salts and react with silver nitrate to prepare silver nano-conductive fillers, and use water as the solvent to use the size of the silver nano-conductive fillers to overcome the coffee ring effect. Achieve low temperature drying.

Benefits of technology

It effectively overcomes the coffee ring effect, reduces production costs and drying temperature, obtains excellent conductivity and convenience, and provides environmentally friendly silver nanoconductive ink for the application of flexible microelectronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116478576B_ABST
    Figure CN116478576B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a silver nano conductive filler that can overcome the coffee ring effect, comprising: mixing a coating agent with ethylene glycol, heating to 100-200°C and maintaining the temperature until the coating agent is completely dissolved, adding an inorganic salt to react for 0-40 minutes, and finally adding silver nitrate to react until the color is gray-green to obtain a product, and washing the product to obtain a silver nano conductive filler. The present invention overcomes the coffee ring effect through the size of the silver nano conductive filler itself, uses water as a solvent, avoids adding environmentally unfriendly solvents such as ethylene glycol and isopropanol to the solvent, and reduces production costs; the present invention also reduces the drying temperature, and only uses a hair dryer to make the cured conductive flexible pattern have excellent conductivity, thereby improving the convenience of use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conductive ink, and in particular relates to a silver nano conductive filler capable of overcoming the coffee ring effect. Background Art

[0002] With the continuous advancement of science and technology, microelectronic devices and flexible electronic devices are becoming more and more needed by people. Printed electronic technology can print the required conductive patterns on the required devices very well. Conductive ink can be used in many fields, such as transparent conductive film (PET), electronic newspaper (EP), curved display screen, wireless intelligent identification electronic tag (RFID), printed circuit board (PCB), thin film sensor (TFS) and solar panel (TFSB), etc. With the trend of green production, energy conservation and emission reduction in social and economic development, conductive ink will definitely become a key material for the sustainable development of printed electronic technology and the electronics industry.

[0003] Conductive ink is composed of conductive fillers and solvents. Conductive fillers generally include carbon nanotubes, conductive polymers, graphene, and metal nanoparticles (copper, silver, and gold). However, since carbon nanotubes and conductive polymers have lower conductivity than metals, metal nanoparticles have become the main filler in conductive inks. Gold is expensive and copper nanoparticles are easily oxidized, making silver nanoparticles the most commonly used conductive filler.

[0004] At present, there are many reports on the research of metal-based conductive inks. Companies such as Flint Ink Company in the United States and ABC Nanotechnology in South Korea have developed commercially available nano-silver conductive inks, but due to the high production cost and complicated process, large-scale application cannot be achieved. Only universities and research institutes in China are conducting research, and it is still in its infancy. Printing silver nano-conductive ink on the substrate is often accompanied by the existence of a coffee ring effect, resulting in the non-conductivity of the middle part of the printed pattern and greater roughness of the edge part. The coffee ring effect refers to the phenomenon that the edge part dries first due to the large energy during the ink drying process, and the ink in the middle part spreads to the outer layer when drying, and finally gathers and dries at the edge. In order to overcome this phenomenon, the ink composed of nanoparticle fillers uses solvents with different surface tensions to keep the nanoparticles evenly dispersed on the substrate through the surface tension. For example, in order to solve the coffee ring effect of silver nanoparticles, many researchers use different solvents (ethylene glycol, isopropanol) to overcome the coffee ring effect. Dongjo Kim (Direct writing of silver conductive patterns: Improvement of film morphology and conductance by controlling solvent compositions) uses ethylene glycol as a solvent for silver nanoparticle conductive ink to overcome the coffee ring effect and achieve good conductivity. However, this will bring about environmental toxicity and high cost. At the same time, the presence of organic matter between nanoparticles increases the sintering temperature, which is generally above 100°C, causing inconvenience in use. Therefore, it is necessary to prepare silver nano conductive ink that can overcome the coffee ring effect, can be dried at low temperature, and is environmentally friendly. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a silver nano-conductive filler that can overcome the coffee ring effect. The silver nano-conductive filler obtained by the method overcomes the inherent coffee ring effect of the silver nano-conductive filler by utilizing its own size, and adopts low-temperature drying, which is environmentally friendly and inexpensive.

[0006] Another object of the present invention is to provide the silver nano conductive filler obtained by the above method.

[0007] Another object of the present invention is to provide a method for preparing silver nano conductive ink.

[0008] The purpose of the present invention is achieved through the following technical solutions.

[0009] A method for preparing a silver nano conductive filler capable of overcoming the coffee ring effect comprises: mixing a coating agent with ethylene glycol, heating to 100-200°C and maintaining the temperature until the coating agent is completely dissolved, adding an inorganic salt to react for 0-40 minutes, and finally adding silver nitrate to react until the color becomes gray-green to obtain a product, and washing the product to obtain the silver nano conductive filler, wherein, by mass, the ratio of the coating agent, the inorganic salt and the silver nitrate is (2-6): (0.1-8): (0.1-10), the ratio of the mass fraction of the coating agent to the volume fraction of the ethylene glycol is (2-6): (1-500), the coating agent is polyvinyl pyrrolidone, hexadecyltrimethylammonium bromide or polyvinyl alcohol, and the inorganic salt is a mixture of one or more of NaCl, FeCl3, NaF and AgNO3.

[0010] In the above technical solution, the washing is performed by adding distilled water and then centrifuging to obtain the solid obtained by centrifugation, wherein the rotation speed of the centrifugation is 1000 to 7000 rpm / min.

[0011] In the above technical solution, the unit of the mass fraction is g, and the unit of the volume fraction is mL.

[0012] The silver nano conductive filler is obtained by the above method.

[0013] A method for preparing silver nano conductive ink comprises the following steps: dispersing the silver nano conductive filler in water to obtain the silver nano conductive ink.

[0014] In the above technical solution, the size of the silver nano conductive filler is 1 to 50 μm.

[0015] In the above technical solution, the ratio of the silver nano conductive filler to water is (1-1000): (1-1000) by mass.

[0016] The silver nano conductive ink obtained by the above preparation method.

[0017] The application of the above silver nano conductive filler in overcoming the coffee ring effect.

[0018] The method for using the silver nano conductive ink comprises: printing or brushing the silver nano conductive ink on a flexible substrate through a printer, drying at a low temperature, and curing on the flexible substrate to form a conductive flexible pattern.

[0019] In the above technical solution, the flexible substrate is photo paper, paper or polyethylene terephthalate (PET).

[0020] In the above technical solution, the low-temperature drying is achieved by using a hair dryer.

[0021] In the above technical solution, the temperature of the low-temperature drying is at least 30°C.

[0022] The silver nano-conductive filler of the present invention has a large size and high quality. During the use of the silver nano-conductive filler, the solvent in the middle has volatilized before it has time to move to the edge after the edge is dried. Therefore, it can be evenly dispersed on the flexible substrate with only water without other solvents, thus overcoming the coffee ring effect. The preparation process of the silver nano-conductive filler uses ethylene glycol as a reducing agent. In the process of preparing the silver nano-conductive filler into silver nano-conductive ink, green and economical water can be used as a solvent, avoiding the addition of environmentally unfriendly solvents such as ethylene glycol and isopropanol to the solvent, and greatly reducing the production cost. The silver nano-conductive filler prepared by the present invention reduces the drying temperature due to its own size, and only a hair dryer is used to make the cured conductive flexible pattern have excellent conductivity, which improves the convenience of use and provides the possibility for the future use of flexible microelectronic devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is the XRD pattern;

[0024] Figure 2a is SEM (400 μm);

[0025] Figure 2b is SEM (50 μm);

[0026] Figure 3a The resistance test of the conductive flexible pattern obtained in Example 1;

[0027] Figure 3b The resistance test of the conductive pattern obtained in Comparative Example 7;

[0028] Figure 4a This is a graph showing the change in sheet resistance of the conductive flexible pattern obtained in Example 3 as a function of the number of printing times (printed on A4 paper);

[0029] Figure 4b This is a graph showing the change in sheet resistance of the conductive flexible pattern obtained in Example 3 as a function of the number of prints (printed on Epson photo paper);

[0030] Figure 5 For SEM;

[0031] Figure 6a is the atomic force microscopy image (10 μm);

[0032] Figure 6b Atomic force microscopy image (10 μm). DETAILED DESCRIPTION

[0033] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0034] The related instruments and equipment used in the specific implementation of the present invention are as follows:

[0035] Inkjet printer: HP DeskJet 1112.

[0036] The drugs used in the specific implementation of the present invention are as follows:

[0037] Coating agent: Aladdin Pharmaceutical Co., Ltd., purity ≥98%;

[0038] Inorganic salt: Aladdin Pharmaceutical Co., Ltd., purity ≥98%;

[0039] Silver nitrate: Aladdin Pharmaceutical Co., Ltd., purity ≥98% (flakes);

[0040] Ethylene glycol: Tianjin Jiangtian Tongyi Technology Co., Ltd., mass fraction> 99.7%;

[0041] Ethanol: Tianjin Jiangtian Tongyi Technology Co., Ltd., mass fraction> 99.7%;

[0042] Isopropyl alcohol: Tianjin Jiangtian Tongyi Technology Co., Ltd., mass fraction> 99.7%;

[0043] Toluene: Tianjin Jiangtian Tongyi Technology Co., Ltd., mass fraction > 99.7%.

[0044] Example 1

[0045] A method for preparing a silver nano conductive filler capable of overcoming the coffee ring effect, comprising:

[0046] In a round-bottom flask, a coating agent and ethylene glycol are mixed, heated to 130°C and kept at a constant temperature until the coating agent is completely dissolved, an inorganic salt is added to react for 10 minutes, and finally silver nitrate is added to react until the color becomes gray-green to obtain a product, and the product is washed to obtain a silver nano conductive filler, wherein the inorganic salt is a mixture of NaCl and FeCl3, the ratio of the mass fraction of the coating agent to the volume fraction of ethylene glycol is 2:100, and the ratio of the coating agent, NaCl, FeCl3 and silver nitrate is 2:0.1:0.1:0.1 by mass fraction, the coating agent is polyvinyl pyrrolidone, the unit of mass fraction is g, and the unit of volume fraction is mL, and washing is performed by adding distilled water and then centrifuging at 3000 rpm / min;

[0047] The purpose of washing is to remove excess coating agent on the surface of the silver nano-conductive filler to obtain silver nano-conductive ink with higher conductivity.

[0048] Silver nano-conductive fillers with a size of 1 to 7 μm are selected and dispersed in water to obtain silver nano-conductive ink, wherein the ratio of the silver nano-conductive fillers to water is 1:100 by weight.

[0049] The obtained silver nano conductive ink is injected into a brush tube with a syringe, and the silver nano conductive ink is brushed on a flexible substrate with a brush, and low-temperature dried at 45° C. for 2 minutes with a hair dryer, and solidified on the flexible substrate to form a conductive flexible pattern with a thickness of 7 μm, wherein the flexible substrate is paper.

[0050] Example 2

[0051] A method for preparing a silver nano conductive filler capable of overcoming the coffee ring effect, comprising:

[0052] In a round-bottom flask, a coating agent and ethylene glycol are mixed, heated to 200°C and kept at a constant temperature until the coating agent is completely dissolved, an inorganic salt is added to react for 8 minutes, and finally silver nitrate is added to react until the color becomes gray-green to obtain a product, and the product is washed to obtain a silver nano conductive filler, wherein the inorganic salt is a mixture of NaCl, FeCl3 and AgNO3, the ratio of the mass fraction of the coating agent to the volume fraction of ethylene glycol is 6:500, and the ratio of the coating agent, NaCl, FeCl3, AgNO3 and silver nitrate is 6:2:2:2:10 by mass fraction, the coating agent is polyvinyl pyrrolidone, the unit of mass fraction is g, and the unit of volume fraction is mL, and washing is performed by adding distilled water and centrifuging at 3500rpm / min;

[0053] Silver nano-conductive fillers with a size of 1 to 7 μm are selected and dispersed in water to obtain silver nano-conductive ink, wherein the ratio of the silver nano-conductive fillers to water is 1:150 by weight.

[0054] The obtained silver nano conductive ink was injected into the ink cartridge of an inkjet printer by using a syringe, and the silver nano conductive ink was printed on a flexible substrate by using an inkjet printer. The ink was dried at a low temperature of 43° C. for 10 minutes by using a hair dryer, and solidified on the flexible substrate to form a conductive flexible pattern with a thickness of 4 μm, wherein the flexible substrate was photo paper.

[0055] Example 3

[0056] A method for preparing a silver nano conductive filler capable of overcoming the coffee ring effect, comprising:

[0057] In a round-bottom flask, a coating agent and ethylene glycol are mixed, heated to 200°C and kept at a constant temperature until the coating agent is completely dissolved, an inorganic salt is added to react for 12 minutes, and finally silver nitrate is added to react until the color becomes gray-green to obtain a product, and the product is washed to obtain a silver nano conductive filler, wherein the inorganic salt is a mixture of NaCl, FeCl3 and AgNO3, the ratio of the mass fraction of the coating agent to the volume fraction of ethylene glycol is 6:300, and the ratio of the coating agent, NaCl, FeCl3, AgNO3 and silver nitrate is 6:2:2:2:5 by mass fraction, the coating agent is polyvinyl pyrrolidone, the unit of mass fraction is g, and the unit of volume fraction is mL, and washing is performed by adding distilled water and then centrifuging at 2500rpm / min;

[0058] Silver nano-conductive fillers with a size of 1 to 7 μm are selected and dispersed in water to obtain silver nano-conductive ink, wherein the ratio of the silver nano-conductive fillers to water is 1:200 by weight.

[0059] The obtained silver nano conductive ink was injected into the ink cartridge of an inkjet printer with a syringe, and the silver nano conductive ink was printed on a flexible substrate by the inkjet printer. A hair dryer was used to low-temperature dry the ink at 40° C. for 5 minutes, and the ink was cured on the flexible substrate to form a conductive flexible pattern, wherein the flexible substrate was A4 paper or Epson photo paper. The conductive flexible pattern was printed on A4 paper 12 times to obtain a thickness of 5 μm, and the conductive flexible pattern was printed on Epson photo paper 9 times to obtain a thickness of 6 μm.

[0060] Example 4

[0061] A method for preparing a silver nano conductive filler capable of overcoming the coffee ring effect, comprising:

[0062] In a round-bottom flask, a coating agent and ethylene glycol are mixed, heated to 130°C and kept at a constant temperature until the coating agent is completely dissolved, an inorganic salt is added to react for 5 minutes, and finally silver nitrate is added to react until the color becomes gray-green to obtain a product, and the product is washed to obtain a silver nano conductive filler, wherein the inorganic salt is a mixture of NaCl and AgNO3, the ratio of the mass fraction of the coating agent to the volume fraction of ethylene glycol is 2:100, and the ratio of the coating agent, NaCl, AgNO3 and silver nitrate is 2:0.1:0.1:0.1 by mass fraction, the coating agent is hexadecyltrimethylammonium bromide, the unit of mass fraction is g, and the unit of volume fraction is mL, and washing is performed by adding distilled water and then centrifuging at 3000 rpm / min;

[0063] Silver nano-conductive fillers with a size of 1 to 7 μm are selected and dispersed in water to obtain silver nano-conductive ink, wherein the ratio of the silver nano-conductive fillers to water is 1:300 by weight.

[0064] The obtained silver nano conductive ink was injected into the ink cartridge of an inkjet printer with a syringe, and the silver nano conductive ink was printed on a flexible substrate by the inkjet printer. A hair dryer was used to dry the ink at 35° C. for 3 minutes, and the ink was cured on the flexible substrate to form a conductive flexible pattern with a thickness of 5 μm, wherein the flexible substrate was PET.

[0065] Example 5

[0066] A method for preparing a silver nano conductive filler capable of overcoming the coffee ring effect, comprising:

[0067] In a round-bottom flask, a coating agent and ethylene glycol are mixed, heated to 200°C and kept at a constant temperature until the coating agent is completely dissolved, an inorganic salt is added to react for 8 minutes, and finally silver nitrate is added to react until the color becomes gray-green to obtain a product, and the product is washed to obtain a silver nano conductive filler, wherein the inorganic salt is a mixture of NaCl and AgNO3, the ratio of the mass fraction of the coating agent to the volume fraction of ethylene glycol is 2:100, and the ratio of the coating agent, NaCl, AgNO3 and silver nitrate is 2:0.1:0.1:0.1 by mass fraction, the coating agent is hexadecyltrimethylammonium bromide, the unit of mass fraction is g, and the unit of volume fraction is mL, and washing is centrifugation at 3500rpm / min after adding distilled water;

[0068] Silver nano-conductive fillers with a size of 1 to 7 μm are selected and dispersed in water to obtain silver nano-conductive ink, wherein the ratio of the silver nano-conductive fillers to water is 1:500 by weight.

[0069] The obtained silver nano conductive ink was injected into the ink cartridge of an inkjet printer with a syringe, and the silver nano conductive ink was printed on a flexible substrate by the inkjet printer. A hair dryer was used to dry the ink at 33° C. for 3 minutes, and the ink was cured on the flexible substrate to form a conductive flexible pattern with a thickness of 5 μm, wherein the flexible substrate was paper.

[0070] Example 6

[0071] A method for preparing a silver nano conductive filler capable of overcoming the coffee ring effect, comprising:

[0072] In a round-bottom flask, a coating agent and ethylene glycol are mixed, heated to 100°C and kept at a constant temperature until the coating agent is completely dissolved, an inorganic salt is added to react for 30 minutes, and finally silver nitrate is added to react until the color becomes gray-green to obtain a product, and the product is washed to obtain a silver nano conductive filler, wherein the inorganic salt is a mixture of NaCl and AgNO3, the ratio of the mass fraction of the coating agent to the volume fraction of ethylene glycol is 2:100, and the ratio of the coating agent, NaCl, AgNO3 and silver nitrate is 2:0.1:0.1:0.1 by mass fraction, the coating agent is polyvinyl pyrrolidone, the unit of mass fraction is g, and the unit of volume fraction is mL, and washing is performed by adding distilled water and centrifuging at 4000 rpm / min;

[0073] Silver nano-conductive fillers with a size of 1 to 7 μm are selected and dispersed in water to obtain silver nano-conductive ink, wherein the ratio of the silver nano-conductive fillers to water is 1:600 ​​by weight.

[0074] The obtained silver nano conductive ink was injected into the ink cartridge of an inkjet printer with a syringe, and the silver nano conductive ink was printed on a flexible substrate by the inkjet printer. A hair dryer was used to dry the ink at 43° C. for 3 minutes, and the ink was cured on the flexible substrate to form a conductive flexible pattern with a thickness of 5 μm, wherein the flexible substrate was photo paper.

[0075] Example 7

[0076] A method for preparing a silver nano conductive filler capable of overcoming the coffee ring effect, comprising:

[0077] In a round-bottom flask, the coating agent and ethylene glycol are mixed, heated to 100°C and kept at a constant temperature until the coating agent is completely dissolved, and then an inorganic salt is added to react for 1 minute, and finally silver nitrate is added to react until the color becomes gray-green to obtain a product, and the product is washed to obtain a silver nano conductive filler, wherein the inorganic salt is a mixture of NaCl and AgNO3, the ratio of the mass fraction of the coating agent to the volume fraction of ethylene glycol is 2:100, and the ratio of the coating agent, NaCl, AgNO3 and silver nitrate is 2:0.1:0.1:0.3 by mass fraction, the coating agent is polyvinyl pyrrolidone, the unit of mass fraction is g, and the unit of volume fraction is mL, and the washing is centrifugation at 2500rpm / min after adding distilled water;

[0078] Silver nano-conductive fillers with a size of 1 to 7 μm are selected and dispersed in water to obtain silver nano-conductive ink, wherein the ratio of the silver nano-conductive fillers to water is 1:1000 by weight.

[0079] The obtained silver nano conductive ink was injected into the ink cartridge of an inkjet printer by using a syringe, and the silver nano conductive ink was printed on a flexible substrate by using an inkjet printer. A hair dryer was used to dry the ink at a low temperature of 35° C. for 3 minutes, and the ink was cured on the flexible substrate to form a conductive flexible pattern with a thickness of 5 μm, wherein the flexible substrate was photo paper.

[0080] Comparative Example 1

[0081] A method for preparing a conductive ink comprises the following steps:

[0082] Step 1, in a round-bottom flask, mix the coating agent and ethylene glycol, heat to 130°C and keep the temperature constant until the coating agent is completely dissolved, then add an inorganic salt to react for 10 minutes, and finally add silver nitrate to react until the color becomes gray-green to obtain a product, wash the product to obtain a silver nano conductive filler, wherein the inorganic salt is a mixture of NaCl and FeCl3, the ratio of the mass fraction of the coating agent to the volume fraction of ethylene glycol is 2:100, and the ratio of the coating agent, NaCl, FeCl3 and silver nitrate is 2:0.1:0.1:0.1 by mass fraction, the coating agent is polyvinyl pyrrolidone, the unit of mass fraction is g, and the unit of volume fraction is mL, and washing is centrifugation at 3000 rpm / min after adding distilled water;

[0083] Step 2, selecting the silver nano-conductive filler with a size of 1 to 7 μm obtained in step 1 and dispersing it in ethanol to obtain a conductive ink, wherein the ratio of the silver nano-conductive filler to the ethanol is 1:100 by mass.

[0084] The obtained conductive ink is injected into a tube of a tube brush with a syringe, and the conductive ink is brushed on a flexible substrate with the brush. It is sintered at 140° C. for 2 minutes using infrared light and solidified on the flexible substrate to form a conductive pattern with a thickness of 7 μm, wherein the flexible substrate is paper.

[0085] Comparative Example 2

[0086] A method for preparing a conductive ink comprises the following steps:

[0087] Step 1, in a round-bottom flask, mix the coating agent and ethylene glycol, heat to 200°C and keep the temperature constant until the coating agent is completely dissolved, then add an inorganic salt to react for 8 minutes, and finally add silver nitrate to react until the color becomes gray-green to obtain a product, wash the product to obtain a silver nano conductive filler, wherein the inorganic salt is a mixture of NaCl, FeCl3 and AgNO3, the ratio of the mass fraction of the coating agent to the volume fraction of ethylene glycol is 6:500, and the ratio of the coating agent, NaCl, FeCl3, AgNO3 and silver nitrate is 6:2:2:2:10 by mass, the coating agent is polyvinyl pyrrolidone, the unit of mass fraction is g, and the unit of volume fraction is mL, and washing is centrifugation at 3500rpm / min after adding distilled water;

[0088] Step 2, selecting the silver nano-conductive filler with a size of 1 to 7 μm obtained in step 1 and dispersing it in ethanol to obtain a conductive ink, wherein the ratio of the silver nano-conductive filler to ethanol is 1:150 by mass.

[0089] The obtained conductive ink is injected into the ink cartridge of an inkjet printer by a syringe, and the conductive ink is printed on a flexible substrate by the inkjet printer. The conductive ink is sintered at 145° C. for 2 minutes using infrared light, and solidified on the flexible substrate to form a conductive pattern with a thickness of 5 μm, wherein the flexible substrate is photo paper.

[0090] Comparative Example 3

[0091] A method for preparing a conductive ink comprises the following steps:

[0092] Step 1, in a round-bottom flask, mix the coating agent and ethylene glycol, heat to 200°C and keep the temperature constant until the coating agent is completely dissolved, then add inorganic salt to react for 12 minutes, finally add silver nitrate to react until the color becomes gray-green to obtain a product, wash the product to obtain a silver nano conductive filler, wherein the inorganic salt is a mixture of NaCl, FeCl3 and AgNO3, the ratio of the mass fraction of the coating agent to the volume fraction of ethylene glycol is 6:300, and the ratio of the coating agent, NaCl, FeCl3, AgNO3 and silver nitrate is 6:2:2:2:5 by mass fraction, the coating agent is polyvinyl pyrrolidone, the unit of mass fraction is g, and the unit of volume fraction is mL, and washing is centrifugation at 2500rpm / min after adding distilled water;

[0093] Step 2, selecting the silver nano-conductive filler with a size of 1 to 7 μm obtained in step 1 and dispersing it in ethanol to obtain a conductive ink, wherein the ratio of the silver nano-conductive filler to ethanol is 1:200 by mass.

[0094] The obtained conductive ink was injected into the ink cartridge of an inkjet printer using a syringe, and the conductive ink was printed on a flexible substrate using the inkjet printer. The conductive ink was sintered at 135° C. for 90 seconds using infrared light, and solidified on the flexible substrate to form a conductive pattern with a thickness of 5 μm, wherein the flexible substrate was PET.

[0095] Comparative Example 4

[0096] A method for preparing a conductive ink comprises the following steps:

[0097] Step 1, in a round-bottom flask, mix the coating agent and ethylene glycol, heat to 130°C and keep the temperature constant until the coating agent is completely dissolved, then add an inorganic salt to react for 5 minutes, and finally add silver nitrate to react until the color becomes gray-green to obtain a product, wash the product to obtain a silver nano conductive filler, wherein the inorganic salt is a mixture of NaCl and AgNO3, the ratio of the mass fraction of the coating agent to the volume fraction of ethylene glycol is 2:100, and the ratio of the coating agent, NaCl, AgNO3 and silver nitrate is 2:0.1:0.1:0.1 by mass fraction, the coating agent is hexadecyltrimethylammonium bromide, the unit of mass fraction is g, and the unit of volume fraction is mL, and washing is centrifugation at 3000rpm / min after adding distilled water;

[0098] Step 2, selecting the silver nano conductive filler with a size of 1 to 7 μm obtained in step 1 and dispersing it in ethylene glycol to obtain a conductive ink, wherein the ratio of the silver nano conductive filler to the ethylene glycol is 1:300 by mass.

[0099] The obtained conductive ink was injected into the ink cartridge of an inkjet printer using a syringe, and the conductive ink was printed on a flexible substrate using the inkjet printer. The conductive ink was sintered at 160° C. for 60 seconds using infrared light, and solidified on the flexible substrate to form a conductive pattern with a thickness of 5 μm, wherein the flexible substrate was PET.

[0100] Comparative Example 5

[0101] A method for preparing a conductive ink comprises the following steps:

[0102] Step 1, in a round-bottom flask, mix the coating agent and ethylene glycol, heat to 200°C and keep the temperature constant until the coating agent is completely dissolved, then add an inorganic salt to react for 8 minutes, and finally add silver nitrate to react until the color becomes gray-green to obtain a product, wash the product to obtain a silver nano conductive filler, wherein the inorganic salt is a mixture of NaCl and AgNO3, the ratio of the mass fraction of the coating agent to the volume fraction of ethylene glycol is 2:100, and the ratio of the coating agent, NaCl, AgNO3 and silver nitrate is 2:0.1:0.1:0.1 by mass fraction, the coating agent is hexadecyltrimethylammonium bromide, the unit of mass fraction is g, and the unit of volume fraction is mL, and washing is centrifugation at 3500rpm / min after adding distilled water;

[0103] Step 2, selecting the silver nano-conductive filler with a size of 1 to 7 μm obtained in step 1 and dispersing it in isopropyl alcohol to obtain a conductive ink, wherein the ratio of the silver nano-conductive filler to the isopropyl alcohol is 1:500 by mass.

[0104] The obtained conductive ink is injected into the ink cartridge of an inkjet printer by using a syringe, and the conductive ink is printed on a flexible substrate by using the inkjet printer. The conductive ink is sintered at 154° C. for 80 seconds using infrared light, and solidified on the flexible substrate to form a conductive pattern with a thickness of 5 μm, wherein the flexible substrate is paper.

[0105] Comparative Example 6

[0106] A method for preparing a conductive ink comprises the following steps:

[0107] Step 1, in a round-bottom flask, mix the coating agent and ethylene glycol, heat to 100°C and keep the temperature constant until the coating agent is completely dissolved, then add an inorganic salt to react for 30 minutes, and finally add silver nitrate to react until the color becomes gray-green to obtain a product, wash the product to obtain a silver nano conductive filler, wherein the inorganic salt is a mixture of NaCl and AgNO3, the ratio of the mass fraction of the coating agent to the volume fraction of ethylene glycol is 2:100, and the ratio of the coating agent, NaCl, AgNO3 and silver nitrate is 2:0.1:0.1:0.1 by mass fraction, the coating agent is polyvinyl pyrrolidone, the unit of mass fraction is g, and the unit of volume fraction is mL, and washing is centrifugation at 4000rpm / min after adding distilled water;

[0108] Step 2, selecting the silver nano-conductive filler with a size of 1 to 7 μm obtained in step 1 and dispersing it in toluene to obtain a conductive ink, wherein the ratio of the silver nano-conductive filler to toluene is 1:600 ​​by mass.

[0109] The obtained conductive ink is injected into the ink cartridge of an inkjet printer by using a syringe, and the conductive ink is printed on a flexible substrate by using the inkjet printer. The conductive ink is sintered at 134° C. for 90 seconds using infrared light, and solidified on the flexible substrate to form a conductive pattern with a thickness of 5 μm, wherein the flexible substrate is photo paper.

[0110] Comparative Example 7

[0111] A method for preparing a conductive ink comprises the following steps:

[0112] Take 1.3g of hexadecyltrimethylammonium bromide and dissolve it in 5ml of deionized water, then add 1.21g of silver nitrate to obtain mixed solution one, take 0.4g of sodium borohydride and dissolve it in 10ml of deionized water to obtain mixed solution two, mix mixed solution one with mixed solution two, add them into a centrifuge tube and centrifuge at a speed of 8000r / min, wash the solid obtained by centrifugation three times with water to obtain a conductive filler, vacuum dry it at 60°C for 10h and then add it to water to obtain a conductive ink, wherein, by mass, the ratio of the dried conductive filler to water is 1:100.

[0113] The obtained conductive ink is injected into the ink injection tube of the brush with a syringe, and the conductive ink is applied to a flexible substrate with the brush. The conductive ink is baked at 156° C. for 5 minutes using infrared light to solidify on the flexible substrate to form a conductive pattern with a thickness of 13 μm, wherein the flexible substrate is paper.

[0114] Through testing, it can be obtained that the conductive flexible patterns obtained in Examples 1 to 7 and the conductive patterns obtained in Comparative Examples 1 to 6 do not have the coffee ring effect, that is, the silver nano conductive filler of the present invention can overcome the coffee ring effect by using organic substances such as ethanol, ethylene glycol, isopropanol or toluene as solvents, and the silver nano conductive ink prepared by using water as solvent can also overcome the coffee ring effect. At the same time, the conductive flexible pattern can be prepared by low-temperature drying with a hair dryer in the embodiment.

[0115] The silver nano-conductive filler obtained in Example 1 was directly dried in an oven at 60° C. for 20 min, and its XRD was tested as follows: Figure 1 As shown by line a in the figure, it can be seen that only the characteristic peak of silver appears, and there is no characteristic peak of silver oxide that blocks the conductive path, which means that even if it is dried in the air, silver oxide will not appear. Silver has good stability and is not easily oxidized. It will have good conductivity when made into a conductive path.

[0116] The silver nano-conductive ink obtained in Example 1 was dropped onto a silicon wafer using a rubber-tipped dropper and dried on a heating table at 30° C. for 5 min in an air environment. The XRD results were as follows: Figure 1 As shown by line b in the figure, it can be seen that only the characteristic peak of silver appears, but there is no silver oxide.

[0117] The silver nano-conductive ink obtained in Example 1 was dropped onto a silicon wafer using a rubber-tipped dropper and dried at 30° C. for 5 min. SEM test was performed. The test results are shown in FIG. Figure 2a and 2b As shown, it can be seen that the silver nano-conductive fillers in the silver nano-conductive ink are linear and have no coffee ring effect.

[0118] Figure 3a This is a resistance test diagram of the conductive flexible pattern obtained in Example 1. Figure 3bThe resistance test diagram of the conductive pattern obtained in Comparative Example 7; Figure 3a and 3b It can be seen that when water is used as the solvent and the concentration of silver nano conductive filler and the conductive filler are the same, although the coating thickness of the granular conductive filler is greater than that of the linear silver nano conductive filler, the resistance of the conductive flexible pattern prepared in Example 1 is only 1Ω, while the resistance of the conductive pattern prepared in Comparative Example 7 is 4Ω. The resistance of the conductive pattern formed by the thick granular conductive filler is 4 times that of the conductive flexible pattern prepared by the linear silver nano conductive filler. This is because the silver nano conductive filler overcomes the coffee ring effect, has no invalid accumulation, and can be evenly spread on the flexible substrate, so that the conductive flexible pattern has a good conductive path.

[0119] Figure 4a This is a graph showing the change in sheet resistance of the conductive flexible pattern obtained in Example 3 as a function of the number of printing times (printed on A4 paper); Figure 4b The square resistance of the conductive flexible pattern obtained in Example 3 varies with the number of printing times (printed on Epson photo paper); Figure 4a and 4b It can be seen that when the volume of silver nano conductive ink used for each printing is the same, the resistance of the silver nano conductive ink drops below 50Ω after printing on A4 paper five times, making the conductivity good. The resistance of the silver nano conductive ink drops below 50Ω after printing on photo paper three times, making the conductivity good. Although the roughness of A4 paper is relatively large, the conductive flexible pattern prepared in Example 3 still has good conductivity.

[0120] The conductive ink obtained in Comparative Example 7 was dropped onto a silicon wafer using a rubber-tipped dropper and dried at 30° C. for 5 min. SEM test was performed. Figure 5 As shown by Figure 5 It can be seen that the conductive filler is in granular form and has an obvious coffee ring effect when water is used as the solvent.

[0121] The silver nano conductive ink obtained in Example 1 and the conductive ink obtained in Comparative Example 7 were diluted 100 times and dropped onto a silicon wafer using a rubber-tipped dropper and dried at 30° C. for 4 minutes. Atomic force microscopy tests were performed. The test results are shown in FIG. Figure 6a and 6b As shown by Figure 6a and 6bIt can be seen that the silver nano conductive filler in the silver nano conductive ink is linear, and the conductive filler in the conductive ink is granular; under the same concentration of the silver nano conductive ink obtained in Example 1 and the conductive ink obtained in Comparative Example 7 and the same drying conditions, after the water evaporates, the silver nano conductive filler is evenly dispersed on the entire silicon wafer substrate with good dispersibility, and the conductive filler moves to the right side of the silicon wafer substrate during the drying process; it is explained that the silver nano conductive ink prepared with water as a solvent for silver nano conductive filler can make the silver nano conductive filler evenly dispersed on the surface of the silicon wafer substrate, overcome the coffee ring effect, so that the conductive flexible pattern prepared with the silver nano conductive ink can form a good conductive path; while the conductive ink prepared with water as a solvent for conductive filler cannot make the conductive filler evenly dispersed on the surface of the silicon wafer substrate, cannot overcome the coffee ring effect, and thus the conductive pattern prepared with the conductive ink cannot form a good conductive path.

[0122] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.

Claims

1. A use of a silver nano conductive filler in a silver nano conductive ink to overcome the coffee ring effect, characterized in that: The silver nano-conductive ink is printed or brushed on a flexible substrate by a printer, dried at low temperature, and solidified on the flexible substrate to form a conductive flexible pattern, wherein the temperature of the low-temperature drying is at least 30° C. The silver nano-conductive ink is a mixture of silver nano-conductive filler and water. The preparation method of the silver nano-conductive filler comprises: mixing a coating agent with ethylene glycol, heating to 100-200° C. and maintaining the temperature until the coating agent is completely dissolved, then adding an inorganic salt to react for 1-40 minutes, and finally adding silver nitrate to react until the color becomes gray-green to obtain a product, washing the product, A silver nano conductive filler is obtained, wherein, in terms of mass fractions, the ratio of the coating agent, the inorganic salt and the silver nitrate is (2-6): (0.1-8): (0.1-10), the ratio of the mass fraction of the coating agent to the volume fraction of the ethylene glycol is 2:100, the unit of the mass fraction is g, the unit of the volume fraction is mL, the coating agent is polyvinyl pyrrolidone, hexadecyltrimethylammonium bromide or polyvinyl alcohol, and the inorganic salt is a mixture of one or more of NaCl, FeCl3, NaF, and AgNO3.

2. The use according to claim 1, characterized in that The washing step is to add distilled water and then centrifuge to obtain the solid obtained by centrifugation, wherein the rotation speed of the centrifuge is 1000-7000RPM.

3. The use according to claim 2, characterized in that: The flexible substrate is paper or polyethylene terephthalate.