A kind of anti-ultraviolet polyester-cotton blended fabric and preparation method thereof

By performing eutectic and acetylation treatments on lignocellulose raw materials, modifying the dispersion of lignin and cellulose in non-polar binders, combined with the addition of nanosilver, the poor dispersion of lignin in UV-resistant fabrics is solved And the coating is easy to crack, which improves the anti-ultraviolet and antibacterial properties of the fabric.

CN116497600BActive Publication Date: 2024-10-01HANGZHOU CHENHAO TEXTILE FINISHING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310503030.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-10-01
Estimated Expiration
2043-05-06

AI Technical Summary

Technical Problem

It is difficult for lignin in existing UV-resistant fabrics to be evenly dispersed in non-polar adhesives, resulting in insufficient UV resistance and easy cracking of the coating.

Method used

By subjecting lignocellulosic raw materials to eutectic treatment and acetylation, lignin and cellulose are stripped and modified so that they are evenly dispersed in the non-polar binder, increasing film-forming toughness, and improving dispersion through an extraction step and compatibility, adding nano-silver to improve antibacterial and anti-UV properties.

Benefits of technology

Significantly improves the UV resistance and durability of UV-resistant fabrics, prevents coating cracking, and enhances the fabric's antibacterial ability and UV resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004214515410000091
    Figure BDA0004214515410000091
  • Figure BDA0004214515410000101
    Figure BDA0004214515410000101
  • Figure BDA0004214515410000102
    Figure BDA0004214515410000102
Patent Text Reader

Abstract

The present application discloses an anti-ultraviolet polyester-cotton blended fabric and a preparation method thereof. The anti-ultraviolet polyester-cotton blended fabric is obtained by treating a polyester-cotton blended fabric substrate with a finishing agent, wherein the finishing agent comprises a lignin solution, anti-ultraviolet particles and a non-polar adhesive in a mass ratio of (4-5): (1-2): (10-15); the lignin solution is obtained by sequentially treating wood fiber powder with a low eutectic treatment, an acetylation treatment and an extraction. The anti-ultraviolet polyester-cotton blended fabric prepared by the present application not only has more outstanding anti-ultraviolet performance, but also has certain antibacterial performance, thereby improving anti-ultraviolet durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of anti-ultraviolet fabrics, and in particular to an anti-ultraviolet polyester-cotton blended fabric and a preparation method thereof. Background Art

[0002] Excessive ultraviolet light will not only cause dyes and colors to change, paper and plastics to age, but also damage human skin, bringing many negative effects. Nowadays, most anti-ultraviolet fabrics are made of non-degradable fossil-based resins such as polyethylene, polypropylene, and polystyrene. These materials will seriously increase carbon dioxide emissions during production and degradation.

[0003] In recent years, research on bio-based anti-ultraviolet materials has continued to emerge, such as lignin, which has good anti-ultraviolet properties. However, when the specially separated lignin is added as a branched aldehyde-phenol polymer to make an anti-ultraviolet film, it is difficult to disperse it homogeneously and stably in a non-polar adhesive due to the difference in polarity, resulting in insufficient anti-ultraviolet performance of the final anti-ultraviolet fabric. Summary of the invention

[0004] In order to solve the problem that lignin in UV-resistant polyester-cotton blended fabric is difficult to be uniformly and stably dispersed in a non-polar adhesive, the present application provides a UV-resistant polyester-cotton blended fabric and a preparation method thereof.

[0005] In a first aspect, the present application provides an anti-ultraviolet polyester-cotton blended fabric, which is obtained by treating a polyester-cotton blended fabric substrate with a finishing agent, wherein the finishing agent comprises a lignin solution, anti-ultraviolet particles and a non-polar adhesive in a mass ratio of (4-5):(1-2):(10-15); the lignin solution is obtained by subjecting wood fiber powder to a low-melting treatment, an acetylation treatment and an extraction in sequence.

[0006] In order to give the fabric sufficient anti-ultraviolet performance, this application uses more anti-ultraviolet particles, which leads to the brittleness of the finishing agent after film formation and the coating cracking phenomenon. Therefore, the present solution needs to solve the dispersion problem of lignin in non-polar adhesives and the problem of coating cracking. In view of this, the scheme of the present application can obtain a lignin solution uniformly dispersed with cellulose and lignin, which can not only improve the anti-ultraviolet performance of the fabric after finishing through lignin, but also use cellulose to make the finishing agent of the polar system have better film-forming toughness, and prevent the cracking of the anti-ultraviolet film layer to a certain extent. Specifically, the present application first treats the wood fiber raw material with a low eutectic method, and can relatively completely peel off lignin and cellulose from the wood fiber raw material. The low eutectic solvent used in the low eutectic method is composed of a hydrogen bond donor and a hydrogen bond acceptor. It is a uniform liquid formed by mixing and heating two substances. The hydrogen bond interaction established between the two components will cause the melting point of the mixture to decrease. The interaction of hydrogen bonds in the low eutectic solvent can not only lower the melting points of the two, but also react with the hydrogen bonds inside the wood fiber raw materials, destroying the original hydrogen bond structure, forming new hydrogen bonds, and promoting the breaking of unstable ether bonds between lignin phenylpropane units. The structure of the wood fiber raw materials is damaged, and lignin and cellulose can be stably stripped out.

[0007] The low eutectic liquid containing lignin and cellulose is then acetylated, and an acetylation agent is added to modify the lignin and cellulose. Acetyl groups are inserted to replace part of the hydroxyl groups, thereby reducing the polarity of lignin and cellulose and improving the compatibility between lignin, cellulose and non-polar adhesives. This allows cellulose and lignin to be better dispersed in the finishing agent, improves the film-forming property of the finishing agent coating, and enhances the durability and UV resistance of the final fabric.

[0008] Finally, the acetylated lignin is extracted to separate the lignin and cellulose with relatively small molecular weight and dispersion coefficient, thereby improving the uniformity of the lignin. This allows the lignin in the finishing agent to have better dispersibility and stability, and to be well compatible with cellulose in the solution, thereby improving the UV resistance of the fabric.

[0009] In addition, the recombinant compatibility of lignin and cellulose is poor, and the exogenous addition of either one cannot make the two compatible. The present application processes the wood fiber powder to simultaneously strip out the lignin and cellulose, ensuring that they are mixed and compatible during the reaction and are not extracted separately, so the two show good compatibility in the finishing agent, which to a certain extent alleviates the problem of poor recombinant compatibility of lignin and cellulose, and effectively improves the film-forming performance and UV resistance of the fabric after finishing.

[0010] Preferably, in the eutectic treatment, the mass ratio of the eutectic solvent to the wood fiber powder is (1-2): (1-3).

[0011] In the eutectic treatment, water is preferably used to dilute the eutectic solvent; more preferably, the mass ratio of water to the eutectic solvent is (1-2):(5-15).

[0012] Each solute of the low eutectic solvent can reduce the melting point of the whole solvent to a level lower than that of each solute through the action of hydrogen bonds. The hydrogen bond donor and hydrogen bond acceptor can be mixed in a certain proportion and stirred into a uniform liquid. The low eutectic solvent is diluted with water and used to treat wood fiber powder, which can destroy the LCC connection between lignin and hemicellulose in the wood fiber powder. The cellulose will also fall off due to the breakage of the connection. The cellulose and lignin are stripped into the solvent. When the low eutectic treatment is carried out according to the mass ratio, the ratio of the stripped lignin and cellulose is increased, which greatly improves the comprehensive improvement of the film-forming property and UV resistance of the finishing agent.

[0013] Preferably, the low eutectic solvent comprises choline chloride and 1,3-butanediol, and the molar ratio of choline chloride to 1,3-butanediol is 1:(3-4).

[0014] By adopting the above technical solution, lignin and cellulose can be stripped and dissolved more effectively. The chloride ions in choline chloride can form hydrogen bonds with the hydroxyl groups between lignin and carbohydrates, destroying the strong hydrogen bonds in the wood fiber powder, strengthening the effect of separating lignin and cellulose, increasing the concentration of lignin and cellulose in the finishing agent, and improving the durability and UV resistance of the fabric.

[0015] Preferably, in the acetylation treatment, the mass ratio of the acetylation agent to the wood fiber powder is (0.2-0.4):(1-2); the acetylation agent includes at least one of acetic anhydride and glacial acetic acid.

[0016] The physical and chemical properties of lignin, cellulose and non-polar adhesives are very different, and it is difficult to disperse and make them compatible in non-polar adhesives. The present application uses an acetylation agent to introduce acetyl groups into lignin to replace a portion of hydroxyl groups, thereby reducing the polarity of lignin and cellulose, allowing lignin to be better dispersed in non-polar adhesives, and making the finished fabric have better UV resistance.

[0017] Preferably, the extractant used in the extraction step includes at least one of ethylene glycol, butanone and acetone; the mass ratio of the extractant to the wood fiber powder is (3-5): (1-2).

[0018] Lignin and cellulose after eutectic treatment are separated by destroying the structure of wood fiber powder by eutectic solvent. The degree of destruction is uncontrollable, and the molecular weight of separated lignin and cellulose varies greatly. If they are used directly to make finishing agents, the density, composition, and properties of the finishing agents will be different, and the uniformity will be affected, and the anti-ultraviolet performance of the fabric will also be reduced. The present application utilizes the different solubility of lignin and cellulose of different molecular weights in different solvents to extract lignin and cellulose of similar molecular weight, so that the lignin and cellulose in the lignin solution have better uniformity and improve the anti-ultraviolet performance of the fabric.

[0019] Using butanone as an extractant can extract lignin with a smaller molecular weight. The smaller the molecular weight of lignin, the smaller its particle size, the better its dispersibility in the solution, and the stronger its adsorption capacity. At the same time, the smaller the particle size, the larger the surface area, the more surface functional groups, the higher the anti-ultraviolet ability, and the anti-ultraviolet performance of the fabric will also be improved. At the same time, cellulose is also easily soluble in butanone and can be extracted together with small molecular weight lignin to maintain good compatibility.

[0020] Preferably, the eutectic treatment of lignin is performed as follows: a eutectic solvent is added to wood fiber powder, heated to 80-100° C., and reacted for 1-2 hours to obtain a lignin eutectic solution.

[0021] By adopting the above technical solution, wood fiber powder is added into an aqueous solution of a low eutectic solvent, heated for reaction, and lignin and cellulose are stripped out.

[0022] Preferably, the acetylation treatment is performed as follows: an acetylation agent is added to the lignin eutectic solution, the temperature is raised to 70-90° C. for reaction, and an acetylated lignin solution is obtained after 2-4 hours.

[0023] By adopting the above technical scheme, the hydroxyl groups of lignin and cellulose are grafted into acetyl groups through acetylation agents, so that the polarity of lignin and cellulose is reduced, and the compatibility and dispersibility between them and non-polar adhesives are better, thereby enhancing the dispersibility of lignin and cellulose in the finishing agent and improving the UV resistance of the fabric.

[0024] Preferably, the acetylated lignin solution is extracted by the following operation: adding an extractant to the acetylated lignin solution, fully dissolving it, and collecting the extract as the lignin solution.

[0025] By adopting the above technical scheme, lignin and cellulose are extracted, and the lignin and cellulose with large differences in size stripped out by the low eutectic are extracted into parts with similar particle size and mass fraction, thereby improving the uniformity and stability of the particles in the finishing agent and enhancing the anti-ultraviolet effect of the fabric.

[0026] Preferably, the finishing agent for preparing the UV-resistant polyester-cotton blended fabric also contains nano-silver; the added amount of the nano-silver is 2-10wt% of the acetylated lignin solution.

[0027] By adopting the above technical solution, the antibacterial effect can be added to the fabric. After low eutectic treatment and acetylation treatment, lignin basically has no antibacterial ability, which has an adverse effect on the durability of clothing and anti-ultraviolet layer. After adding 5-10wt% of nano silver mass dispersant to disperse nano silver in the lignin solution, on the one hand, the antibacterial ability of the fabric is improved; on the other hand, after adding the adhesive, due to the light transmittance of the adhesive, the anti-ultraviolet performance of the anti-ultraviolet finishing agent will decrease, and the uniform dispersion of nano silver particles in the finishing agent will reduce the light transmittance of the impregnating agent, and further improve the anti-ultraviolet performance of the fabric.

[0028] In a second aspect, the present application provides a method for preparing an anti-ultraviolet polyester-cotton blended fabric, comprising the following steps: finishing agent: mixing a lignin solution, anti-ultraviolet particles and a non-polar adhesive, and stirring them uniformly to obtain a finishing agent;

[0029] Finishing: immerse the fabric base material in a finishing agent at 40-60°C for 30-40 minutes, take it out and dry it to shape it, so as to obtain an anti-ultraviolet polyester-cotton blended fabric.

[0030] By adopting the above technical scheme, the fabric base material is first woven in a satin manner, which can better block the harm of ultraviolet light to the human body at the physical level. Then the prepared lignin solution is mixed with an aqueous adhesive, arranged on the surface of the fabric, and dried in an environment of 70-80°C, and shaped in an environment of 100-130°C. Then, it is soaked in warm water of 30-40°C, and a central detergent is added. After 30-60 minutes, it is rinsed with clean water, repeated 2-3 times and dried naturally, and an anti-ultraviolet polyester-cotton blended fabric can be obtained.

[0031] Preferably, the non-polar adhesive is a methyl methacrylate solution adhesive, and the added amount is 40-50wt% of the lignin solution.

[0032] Preferably, the methyl methacrylate solution adhesive is a mixture of polymethacrylate and any one of ketones; and the content of polymethyl methacrylate is 15-25%.

[0033] More preferably, the fabric substrate is satin weave.

[0034] More preferably, the bath ratio of the finishing agent to the fabric substrate is (8-10):1.

[0035] In summary, this application has the following beneficial effects:

[0036] 1. In the present application, lignin and cellulose are stripped and modified together by subjecting the wood fiber raw materials to low-melting treatment and acetylation treatment, and finally extracted together. Since lignin and cellulose are always fused together and are not extracted separately, the problem of poor compatibility of the two in re-compounding is alleviated, so that the two can be evenly dispersed and well fused in the finishing agent, thereby improving the anti-ultraviolet performance of the fabric.

[0037] 2. After the lignin solution prepared in the present application is subjected to low-melting treatment and acetylation treatment, the polarity of lignin and cellulose is reduced, so that it can be better dispersed in the non-polar adhesive, increasing the UV resistance of the fabric. At the same time, the presence of cellulose improves the problem of poor film-forming performance caused by anti-UV particles.

[0038] 3. The present application extracts cellulose and lignin of similar molecular weight by extracting acetylated lignin, so that the lignin in the final finishing agent is uniform, thereby better improving the anti-ultraviolet performance of the fabric.

[0039] 4. The present application adds nano-silver into the lignin solution, so that the fabric not only increases the antibacterial ability to a certain extent, but also further improves the anti-ultraviolet performance. DETAILED DESCRIPTION

[0040] Preparation example of lignin solution

[0041] Preparation Example 1: A lignin solution is prepared according to the following steps:

[0042] Pretreatment: 200 g of poplar sawdust (particle size 0.05-1 mm) was passed through a 0.1 mm sieve to obtain wood fiber powder.

[0043] Preparation of solvent: 10 mol of choline chloride and 30 mol of 1,3-butanediol were mixed, and heated and stirred in a water bath at 80° C. until the mixture became colorless and transparent to obtain a low eutectic solvent.

[0044] Eutectic: 25 ml of eutectic solvent was mixed with 200 ml of distilled water, and heated with 50 g of wood fiber powder in a three-necked flask at 95° C. for 1 hour to obtain a lignin eutectic solution.

[0045] Acetylation: 40 g of acetic anhydride was added to 200 g of lignin eutectic solution, and the temperature was raised to 80° C. to react. After 2 hours, an acetylated lignin solution was obtained.

[0046] Extraction: Put 50g of acetylated lignin solution into 1000ml of butanone, stir at room temperature for 2 hours, and collect the extraction solution as the lignin solution.

[0047] Silver loading: 10 g of nanosilver was dispersed in 200 g of lignin solution, and 1 g of sodium dodecyl sulfate was added as a dispersant. After stirring for 2 hours, a silver-loaded lignin solution was obtained.

[0048] Preparation Example 2: A lignin solution was prepared according to the following steps:

[0049] Pretreatment: 200 g of poplar sawdust (particle size 0.05-1 mm) was passed through a 0.1 mm sieve to obtain wood fiber powder.

[0050] Preparation of solvent: 10 mol of choline chloride and 30 mol of 1,3-butanediol were mixed, and heated and stirred in a water bath at 80° C. until the mixture became colorless and transparent to obtain a low eutectic solvent.

[0051] Eutectic: 15 ml of eutectic solvent was mixed with 75 ml of distilled water, and heated with 50 g of wood fiber powder at 95° C. for 1 hour in a three-necked flask to obtain a lignin eutectic solution.

[0052] Modification: 80 g of acetic anhydride was added to 200 g of lignin eutectic solution, and the temperature was raised to 80° C. to react. After 2 hours, an acetylated lignin solution was obtained.

[0053] Extraction: Put 50g of acetylated lignin solution into 1000ml of butanone, stir at room temperature for 2 hours, and collect the extraction solution as the lignin solution.

[0054] Silver loading: 10 g of nanosilver was dispersed in 200 g of lignin solution, and 1 g of sodium dodecyl sulfate was added as a dispersant. After stirring for 2 hours, a silver-loaded lignin solution was obtained.

[0055] Preparation Example 3: A lignin solution was prepared according to the following steps:

[0056] Pretreatment: 200 g of poplar sawdust (particle size 0.05-1 mm) was passed through a 0.1 mm sieve to obtain wood fiber powder.

[0057] Preparation of solvent: 10 mol of choline chloride and 30 mol of 1,3-butanediol were mixed, and heated and stirred in a water bath at 80° C. until the mixture became colorless and transparent to obtain a low eutectic solvent.

[0058] Eutectic: 30 ml of eutectic solvent was mixed with 450 ml of distilled water, and heated with 50 g of wood fiber powder at 95° C. for 1 hour in a three-necked flask to obtain a lignin eutectic solution.

[0059] Modification: Add 20 g of acetic anhydride to 200 g of lignin eutectic solution, heat to 80° C. for reaction, and after 2 hours, obtain an acetylated lignin solution.

[0060] Extraction: Put 50g of acetylated lignin solution into 1000ml of butanone, stir at room temperature for 2 hours, and collect the extraction solution as the lignin solution.

[0061] Silver loading: 10 g of nanosilver was dispersed in 200 g of lignin solution, and 0.5 g of sodium dodecyl sulfate was added as a dispersant. After stirring for 2 hours, a silver-loaded lignin solution was obtained.

[0062] Preparation Example 4 is a lignin solution, which is different from Preparation Example 1 in that no nanosilver is added to the finishing agent, that is, no silver loading step is performed in the preparation of the lignin solution.

[0063] Preparation Example 5, a lignin solution, is different from Preparation Example 1 in that an equal amount of citric acid is used in place of choline chloride, and an equal amount of ethylene glycol is used in place of 1,3-butanediol in the preparation solvent.

[0064] Preparation Example 6, a lignin solution, is different from Preparation Example 1 in that, when preparing the solvent, the molar ratio of choline chloride to 1,3-butanediol is 1:6.

[0065] Preparation Example 7, a lignin solution, is different from Preparation Example 1 in that an equal amount of ethylene glycol is used instead of butanone in the extraction step.

[0066] Preparation Example 8, a lignin solution, is different from Preparation Example 1 in that an equal amount of acetone is used instead of butanone in the extraction step.

[0067] Preparation Example 9, a lignin solution, is different from Preparation Example 1 in that no extraction step is provided.

[0068] Preparation Example 10: A lignin solution was prepared according to the following steps:

[0069] Pretreatment: 200 g of poplar sawdust (particle size 0.05-1 mm) was passed through a 0.1 mm sieve to obtain wood fiber powder.

[0070] Modification: 40 g of acetic anhydride was added to 200 g of lignin eutectic solution, and the temperature was raised to 80° C. to react, and an acetylated lignin solution was obtained after 2 hours.

[0071] Extraction: Put 50g of acetylated lignin solution into 1000ml of butanone, stir at room temperature for 2 hours, and collect the extraction solution as the lignin solution.

[0072] Silver loading: 10 g of nanosilver was dispersed in 200 g of lignin solution, and 1 g of sodium dodecyl sulfate was added as a dispersant. After stirring for 2 hours, a silver-loaded lignin solution was obtained.

[0073] Preparation Example 11, a lignin solution is prepared according to the following steps:

[0074] Pretreatment: 200 g of poplar sawdust (particle size 0.05-1 mm) was passed through a 0.1 mm sieve to obtain wood fiber powder.

[0075] Preparation of solvent: 10 mol of choline chloride and 30 mol of 1,3-butanediol were mixed, and heated and stirred in a water bath at 80° C. until the mixture became colorless and transparent to obtain a low eutectic solvent.

[0076] Eutectic: 25 ml of eutectic solvent was mixed with 200 ml of distilled water, and heated with 50 g of wood fiber powder at 95° C. for 1 hour in a three-necked flask to obtain a lignin eutectic solution.

[0077] Extraction: Put 50g of lignin eutectic solution into 1000ml of butanone, stir at room temperature for 2 hours, and collect the extraction solution as the lignin solution.

[0078] Silver loading: 10 g of nanosilver was dispersed in 200 g of lignin solution, and 1 g of sodium dodecyl sulfate was added as a dispersant. After stirring for 2 hours, a silver-loaded lignin solution was obtained.

[0079] Preparation Example 12, a lignin solution was prepared according to the following steps:

[0080] 50g of lignin (Hubei Hanwei Chemical HW010425) was dissolved in 1000ml of butanone, 200g was added with 10g of nanosilver and 1g of sodium dodecyl sulfate, and the silver-loaded lignin solution was obtained after stirring for 2 hours.

[0081] Example

[0082] Example 1, an anti-ultraviolet polyester-cotton blended fabric, is prepared according to the following steps:

[0083] Adhesive: 100 g of polymethyl methacrylate was dissolved in 400 g of butanone, and the mixture was stirred and reacted for 2 hours to obtain a non-polar adhesive.

[0084] Finishing agent: 250 g of the lignin solution prepared in Preparation Example 1, 100 g of zinc oxide and 700 g of a non-polar adhesive were mixed and stirred to obtain a finishing agent.

[0085] Finishing: The satin-woven polyester-cotton blended fabric substrate is immersed in a 50°C finishing agent for 30 minutes, taken out and dried for setting at a drying temperature of 80°C and a setting temperature of 130°C, then immersed in 30°C water and added with calcium dodecylbenzene sulfonate, rinsed with clean water after half an hour, repeated the immersion and rinsing twice and then dried naturally to obtain an anti-UV polyester-cotton blended fabric.

[0086] Example 2, an anti-ultraviolet polyester-cotton blended fabric, is prepared according to the following steps:

[0087] Adhesive: 100 g of polymethyl methacrylate was dissolved in 400 g of butanone, and the mixture was stirred and reacted for 2 hours to obtain a non-polar adhesive.

[0088] Finishing agent: 250 g of the lignin solution prepared in Preparation Example 2, 120 g of zinc oxide and 500 g of a non-polar adhesive were mixed and stirred evenly to obtain a finishing agent.

[0089] Finishing: The satin-woven polyester-cotton blended fabric substrate is immersed in a 50°C finishing agent for 30 minutes, taken out and dried for setting at a drying temperature of 80°C and a setting temperature of 130°C, then immersed in 30°C water and added with calcium dodecylbenzene sulfonate, rinsed with clean water after half an hour, repeated the immersion and rinsing twice and then dried naturally to obtain an anti-UV polyester-cotton blended fabric.

[0090] Embodiment 3, a kind of UV-resistant polyester-cotton blended fabric is prepared according to the following steps:

[0091] Adhesive: 100 g of polymethyl methacrylate was dissolved in 400 g of butanone, and the mixture was stirred and reacted for 2 hours to obtain a non-polar adhesive.

[0092] Finishing agent: 250 g of the lignin prepared in Preparation Example 3 was dissolved.

[0093] Finishing: The satin-woven polyester-cotton blended fabric substrate is immersed in a 50°C finishing agent for 30 minutes, taken out and dried for setting, the drying temperature is 80°C, the setting temperature is 130°C, then immersed in 30°C water, and calcium dodecylbenzene sulfonate is added, rinsed with clean water after half an hour, repeated soaking and rinsing twice, and naturally dried to obtain the UV-resistant polyester-cotton blended fabric.

[0094] Example 4, an anti-ultraviolet polyester-cotton blended fabric, is different from Example 1 in that an equal amount of the lignin solution prepared in Preparation Example 4 is used in the finishing agent step instead of the silver-loaded lignin solution prepared in Preparation Example 1.

[0095] Example 5, an anti-ultraviolet polyester-cotton blended fabric, is different from Example 1 in that an equal amount of the lignin solution prepared in Preparation Example 5 is used in place of the lignin solution prepared in Preparation Example 1 in the finishing agent step.

[0096] Example 6, an anti-ultraviolet polyester-cotton blended fabric, is different from Example 1 in that an equal amount of the lignin solution prepared in Preparation Example 6 is used in the finishing agent step instead of the lignin solution prepared in Preparation Example 1.

[0097] Example 7, an anti-ultraviolet polyester-cotton blended fabric, is different from Example 1 in that an equal amount of the lignin solution prepared in Preparation Example 7 is used in the finishing agent step instead of the lignin solution prepared in Preparation Example 1.

[0098] Example 8, an anti-ultraviolet polyester-cotton blended fabric, is different from Example 1 in that an equal amount of the lignin solution prepared in Preparation Example 8 is used in the finishing agent step instead of the lignin solution prepared in Preparation Example 1.

[0099] Example 9, an anti-ultraviolet polyester-cotton blended fabric, is different from Example 1 in that an equal amount of the lignin solution prepared in Preparation Example 9 is used in the finishing agent step instead of the lignin solution prepared in Preparation Example 1.

[0100] Comparative Example

[0101] Comparative Example 1 is an anti-ultraviolet polyester-cotton blended fabric, which is different from Example 1 in that an equal amount of the lignin solution prepared in Preparation Example 10 is used in the finishing agent step instead of the lignin solution prepared in Example 1.

[0102] Comparative Example 2 is an anti-ultraviolet polyester-cotton blended fabric. The difference from Example 1 is that an equal amount of the lignin solution prepared in Preparation Example 11 is used in the finishing agent step instead of the lignin solution prepared in Example 1.

[0103] Comparative Example 3, an anti-ultraviolet polyester-cotton blended fabric, is different from Example 1 in that an equal amount of the lignin solution prepared in Preparation Example 12 is used in the finishing agent step instead of the lignin solution prepared in Example 1.

[0104] Performance testing

[0105] Test 1: Test method for UV resistance of fabrics: According to the provisions of GB / T 18830-2009 “Evaluation of UV resistance of textiles”, the UV protection factor UPF and UVA transmittance of the UV-resistant polyester-cotton blended fabrics of Examples 1-10 and Comparative Examples 1-3 were tested. The test results are shown in Table 1.

[0106] Test 2: Antibacterial property test of fabrics Test method: According to GB / T20944.32008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method", the antibacterial property of the anti-ultraviolet polyester-cotton blended fabrics of Examples 1-10 and Comparative Examples 1-3 was tested. The test bacteria were: Escherichia coli ATCC25922 and Staphylococcus aureus ATCC6538. The test results are shown in Table 1.

[0107] Experiment 3: Determination of molecular mass of lignin Experimental method: The lignin solutions obtained in Preparation Example 1, Preparation Example 10 and Preparation Example 11 were rotary evaporated, vacuum dried, and then the relative molecular masses were determined by mass spectrometry. The test results are shown in Table 2.

[0108] Test 4: Test method for flexibility of fabric coating: According to GB / T1731-2020 "Determination of flexibility of paint films and putty films", the flexibility of the finishing agents in Examples 1-10 and Comparative Examples 1-3 after film formation was tested. The test results are expressed as the minimum shaft rod diameter at which no cracks or peeling of the coating are observed at least twice, as shown in Table 1.

[0109] Table 1. Anti-ultraviolet and antibacterial properties of anti-ultraviolet polyester-cotton blended fabrics

[0110]

[0111]

[0112] Table 2. Relative molecular weight of lignin

[0113]

[0114] Analysis of test results:

[0115] 1. Combining Examples 1-9 and Comparative Examples 1-3 with Table 1, it can be seen that the present application improves the anti-ultraviolet performance of the anti-ultraviolet polyester-cotton blended fabric and the flexibility of the fabric coating by processing the wood fiber raw material and directly adding exogenous lignin. The reason may be that the lignin and cellulose in the lignin solution directly obtained by processing the wood fiber raw material are not separated, and there is no problem of re-combination. Compared with the extracted lignin and cellulose, it has higher compatibility and can be better dispersed in the impregnating agent in a homogeneous and stable manner. Lignin improves the anti-ultraviolet performance of the fabric, and cellulose improves the film-forming property of the finishing agent, making the fabric coating less likely to crack and increasing the flexibility and durability of the fabric coating.

[0116] 2. Combining Examples 1-9 and Comparative Examples 1-3 with Table 1, it can be seen that the present application can improve the UV resistance of fabrics by subjecting wood fiber materials to low-melting treatment, acetylation treatment and extraction in sequence. The reason may be that lignin and cellulose are first stripped by low-melting treatment, then the polarity of lignin is reduced by acetylation treatment, the dispersibility of lignin in non-polar adhesives is increased, and finally the uniformity of lignin and cellulose in the finishing agent is improved by extraction, thereby improving the UV resistance of the anti-UV coating.

[0117] 3. Combining Example 1, Example 7-9, Preparation Example 1, Preparation Example 7-9 and Table 1 and Table 2, it can be seen that the present application uses butanone to extract acetylated lignin, and the obtained lignin solution can improve the UV resistance of the fabric. The reason may be that butanone has better solubility for lignin with a smaller mass fraction than other solvents, and can extract smaller lignin, and smaller lignin has more surface active groups and has better dispersibility in the finishing agent, thereby improving the UV resistance of the fabric.

[0118] 4. It can be seen from Examples 1-4 and Table 1 that the present application not only makes the anti-ultraviolet coating have antibacterial properties but also improves the anti-ultraviolet performance by carrying silver on the lignin solution. The reason may be that after adding nanosilver, nanosilver first has a strong inhibitory effect on bacteria, and secondly, nanosilver, as a nanoparticle, can reduce the light transmittance of the impregnant, block the invasion of ultraviolet light, and effectively improve the performance and durability of the anti-ultraviolet coating.

[0119] 5. Combining Example 1, Example 5 and Example 6 with Table 1, it can be seen that the present application effectively improves the effect of the low eutectic treatment by using choline chloride and 1,3-butanediol to prepare a low eutectic solvent. The reason may be that the use of choline chloride and 1,3-butanediol in the preparation of the low eutectic solvent can more completely extract and dissolve lignin than other solvents, thereby improving the dispersibility of lignin in the anti-ultraviolet coating, thereby improving the anti-ultraviolet performance.

[0120] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An anti-ultraviolet polyester-cotton blended fabric, obtained by finishing a polyester-cotton blended fabric substrate with a finishing agent, characterized in that: The finishing agent comprises a lignin solution, anti-ultraviolet particles and a non-polar adhesive in a mass ratio of (4-5): (1-2): (10-15); the lignin solution is obtained by sequentially subjecting wood fiber powder to a low eutectic treatment, an acetylation treatment and an extraction; In the eutectic treatment, the mass ratio of the eutectic solvent to the wood fiber powder is (1-2): (1-3); the eutectic solvent is choline chloride and 1,3-butanediol in a molar ratio of 1: (3-4); the eutectic treatment operation is as follows: adding the eutectic solvent to the wood fiber powder, heating to 80-100° C., and reacting for 1-2 hours to obtain a lignin eutectic solution; In the acetylation treatment, the mass ratio of the acetylation agent and the wood fiber powder is (0.2-0.4): (1-2); the acetylation agent includes at least one of acetic anhydride and glacial acetic acid; the acetylation treatment operation is as follows: adding the acetylation agent to the lignin eutectic solution, stirring evenly, heating to 70-90°C for reaction, and obtaining an acetylated lignin solution after 2-4 hours; The extractant used in the extraction step includes at least one of ethylene glycol, butanone, and acetone; the mass ratio of the extractant to the wood fiber powder is (3-5): (1-2); the extraction step is performed as follows: adding the extractant to the acetylated lignin solution, fully dissolving it, and collecting the extract as the lignin solution.

2. The UV-resistant polyester-cotton blended fabric according to claim 1, characterized in that: The finishing agent also contains nano silver, and the added amount of the nano silver is 2-10wt% of the lignin solution.

3. The UV-resistant polyester-cotton blended fabric according to any one of claims 1-2, characterized in that: The preparation method comprises the following steps: Finishing agent: Mix the lignin solution, the anti-ultraviolet particles and the non-polar adhesive, stir evenly, and obtain a finishing agent; Finishing: immerse the fabric base material in a finishing agent at 40-60°C for 30-40 minutes, take it out and dry it to shape it, so as to obtain an anti-ultraviolet polyester-cotton blended fabric.