A kind of waste recycled bricks from construction site of all-underground transportation engineering and preparation method thereof

By using the excavated slag in underground transportation projects and recycled materials and waste slurry water that temporarily supports the concrete enclosure structure, recycled bricks without the need for cement and lime are prepared, which solves the dust in waste treatment and recycling in underground transportation projects. The problem of high cost has achieved efficient and low-cost resource utilization and environmental protection effects.

CN116514463BActive Publication Date: 2024-11-05CHINA RAILWAY NO 2 ENG GROUP CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310459289.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-05
Estimated Expiration
2043-04-26

AI Technical Summary

Technical Problem

In the construction of urban underground transportation projects, there are problems of dust problems, high usage of cement and lime, high cost and low resource utilization, making it difficult to achieve full-component resource utilization.

Method used

Use the excavated slag and temporary support concrete enclosure structure to cut and remove waste slurry water from the recycled material and recycled material processing process, prepare recycled bricks through wet process, and use unhydrated cement particles and hydrated products as cementitious agents to achieve no need for additional addition The cementing and hardening of cement and lime directly uses waste slurry water as the cementing material.

Benefits of technology

It has achieved efficient resource utilization of waste on site of underground transportation engineering construction, saved raw materials and costs, reduced environmental pollution, and the performance of recycled bricks meets the use requirements.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a fully underground traffic engineering construction site waste recycled brick and a preparation method thereof, belonging to the technical field of underground traffic engineering construction waste recycling. The raw materials for preparing the recycled brick include, by mass percentage, 50%-60% of excavation slag, 28%-40% of recycled sand from cutting and removing temporary supporting concrete beams and columns, and 8%-15% of recycled sand sand making waste slurry water from cutting and removing temporary supporting concrete beams and columns. The concrete of the temporary supporting concrete beams and columns has a service time of ≤1 year before cutting and removing. The recycled brick is obtained by mixing the above raw materials, spirally extruding and then subjecting to solar energy curing. The invention utilizes the viscoplasticity of clay minerals in the slag; on the other hand, gives full play to the mechanical properties and potential gelling property of short-term service concrete, so that the fully underground traffic engineering construction site waste recycled brick can be obtained without using cement, lime, natural aggregate and fresh mixing water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of underground transportation engineering construction waste recycling, and specifically relates to a fully underground transportation engineering construction site waste recycling brick and a preparation method thereof. Background Art

[0002] The construction process of urban underground transportation projects includes: open / cover excavation and tunneling of tunnels and passages. In order to ensure the progress of excavation / tunneling, the safety of construction personnel, the placement of construction machinery, and reduce the impact on the traffic of people and vehicles in the surrounding area, temporary supporting concrete enclosure structures are built in the open / cover construction space, including temporary supporting concrete beams, columns, retaining walls, etc. After the excavation, tunneling and its ancillary projects are completed, the temporary supporting concrete enclosure structure is cut and removed, and the construction of permanent supporting enclosure structure, other main structure construction and ancillary projects are carried out. Excavation and tunneling and the cutting and removal of temporary supporting concrete enclosure structures have become the two links with the largest waste emissions in the construction of urban underground transportation projects.

[0003] During the excavation and tunneling process, a large amount of slag is generated. For conventional ground transportation projects, the slag is mainly stabilized and then backfilled into the roadbed. However, the volume of backfill in the foundation of underground transportation projects is relatively small, and most of the excavation slag needs to be transported out for treatment and disposal. Temporary support and enclosure structures are mostly reinforced concrete structures, and the concrete strength grade is the same or similar to that of permanent support and enclosure structures. During the formal construction of the main structure of the project, the temporary support and enclosure structure needs to be cut and dismantled in advance in steps. After the steel bars are roughly broken and separated on site, the remaining inorganic non-metallic waste is either transported out for treatment and disposal as general construction waste, or transported to a processing plant for further processing into recycled sand and gravel aggregates. At present, the production process of recycled aggregate from waste concrete is mainly divided into two types: dry process and wet process. The dry process has more serious dust emission, and the recycled coarse and fine aggregates of waste concrete have a higher powder content, which affects subsequent utilization. The wet process can not only remove dust and reduce dust, but also wash away the fine powder in the recycled coarse and fine aggregates. The processing site environment is good and the performance of the recycled aggregates is better. Most urban underground transportation projects are located in urban areas, and temporary support and maintenance structure waste concrete processing sites are also mostly located near construction sites. Considering many aspects such as reducing dust, temporary support concrete recycling processing mostly uses wet processes. However, wet processes consume a lot of water and generate a large amount of waste slurry. At present, waste slurry from recycled aggregate processing mostly uses sedimentation, flocculation, and filter press separation processes to achieve solid-liquid separation, and water is recycled, while filter press sludge is transported out for landfill.

[0004] In fact, slag can be added to shale to produce sintered bricks / blocks, but the sintered products industry such as bricks, tiles and blocks has high energy consumption, high pollution and high CO2 emissions, which is inconsistent with the green and low-carbon development direction of the industry. Excavation slag contains a high amount of clay minerals. After adding auxiliary materials and cement, lime and other cementitious materials or activators, it can be used to produce unfired bricks / blocks, but such products generally have the problem of high cementitious material and activator usage and high cost, and the economic benefits are not enough to support production and use.

[0005] In view of this, it is necessary to design a resource product and preparation method for waste from urban underground transportation engineering construction sites, including excavation debris, recycled materials from cutting and demolition of temporary supporting concrete enclosure structures, and waste slurry water from the processing of recycled materials, so that all components can be utilized as resources. Summary of the invention

[0006] In order to overcome the problems existing in the background technology, the present invention provides a fully underground transportation engineering construction site waste recycled brick and a preparation method thereof, which utilizes the viscoplasticity of clay minerals in the slag; on the other hand, it gives full play to the mechanical properties and potential cementitiousness of short-term service concrete, thereby obtaining a fully underground transportation engineering construction site waste recycled brick without using cement, lime, natural aggregate and fresh mixing water.

[0007] To achieve the above object, the present invention is implemented through the following technical solutions:

[0008] The said fully underground transportation engineering construction site waste recycled bricks, the preparation raw materials used include, by mass percentage: 50%~60% excavation debris, 28%~40% recycled sand from cutting and dismantling temporary support concrete beams and columns, and 8%~15% waste slurry water from cutting and dismantling temporary support concrete beams and columns; the said excavation debris is produced by open or dark excavation of tunnels by tunnel boring machines / shield machines, the particle size of the excavation debris is less than 2mm, and the moisture content is 8-12%; the concrete of the said temporary support concrete beams and columns has a service life of ≤1 year before cutting and dismantling.

[0009] Furthermore, the regenerated sand for temporary supporting concrete beams and columns is made from concrete blocks cut and removed from temporary supporting concrete beams and columns at the construction site, crushed and recycled steel, and then prepared using a wet sand making process. The moisture content of the regenerated sand is 4-6%, and the physical and chemical indicators meet the requirements of Grade 1 distribution area and Class II medium sand specified in GB / T 25176 "Regenerated Fine Aggregate for Concrete and Mortar".

[0010] Furthermore, the waste slurry water for making recycled sand from temporary supporting concrete beams and columns is the waste slurry water discharged from the process of preparing recycled sand by wet sand making process after the temporary supporting concrete beams and columns at the project site are cut and dismantled, concrete blocks are crushed and steel is recycled. The waste slurry water is collected in a collection tank and pumped into a mixing tank by a mud pump, where it is stirred and concentrated to make the solid content of the waste slurry water reach 10-20%, the fineness of solid particles in the waste slurry water ≤0.15 mm, and more than 90% of the solid particles ≤0.075 mm.

[0011] The method for preparing the recycled bricks from waste at the construction site of the fully underground transportation project comprises the following steps:

[0012] S1 Excavation waste soil, regenerated sand and waste slurry water are measured separately;

[0013] S2 Add the materials into a vacuum clay mixer and mix them to obtain a mixture;

[0014] S3 mixed material is input into the screw extruder for extrusion molding;

[0015] S4 extrusion blocks are directly cut into green pieces online;

[0016] S5 green bricks are stacked and cured in a solar curing room, thus preparing recycled bricks from waste at the construction site of the fully underground transportation project.

[0017] Furthermore, the curing temperature of step S5 is 30-50 degrees Celsius, and the curing time is greater than 28 days.

[0018] Beneficial effects of the present invention:

[0019] Temporary support concrete enclosure structures have a short service life and generally need to be cut and demolished in about one year. Compared with ordinary waste concrete, the concrete for cutting and demolishing temporary support enclosure structures has a higher content of unhydrated cement particles and hydration products Ca (OH) 2. After being ground, it has hydration properties and can play a similar role to cement and lime. Therefore, it can be used as a cementitious stabilizer for slag waste.

[0020] The present invention utilizes the temporary support enclosure structure to cut and dismantle the waste concrete, which has a short service life and contains a large number of unhydrated cement particles and hydration products Ca (OH)2, which have potential cementitious properties and lime excitation effects, but need to be further ground to exert the above-mentioned effects. In the wet sand making process of the waste concrete regenerated by cutting and dismantling the temporary support enclosure structure, fine particles ≤0.15 mm (and most of the fine particles have a particle size of ≤0.075 mm) mostly enter the waste slurry water, and its particle fineness is close to the size of lime or cement particles, that is to say, the waste slurry water can be directly used as cement slurry and lime slurry without further grinding. The present invention utilizes this point and directly replaces the cementitious materials and mixing water of traditional recycled bricks with waste slurry water, truly making the best use of everything.

[0021] The unhydrated cement particles in the waste slurry will continue to hydrate during the curing process of the recycled bricks, and their hydration products and the original cement hydration product Ca (OH)2 in the slurry can react with the active SiO2 and Al2O3 in the excavation slag to form a cementitious system. Therefore, the present invention does not need to further add cement, lime or other stimulants and other external modified materials, and the recycled bricks can still be cemented and hardened to form a higher strength, so that the raw materials of the recycled bricks are all waste, saving raw materials, costs and protecting the environment.

[0022] Recycled sand comes from waste concrete cut and demolished from temporary support and maintenance structures. It also contains unhydrated cement particles and hydration product Ca (OH)2. In the crushing and sand making process, unhydrated cement particles and hydration product Ca (OH)2 are partially exposed, which makes the surface of the regenerated sand particles have cementing activity and activity stimulation effect. When the regenerated sand particles come into contact with the slag on their surface, volcanic ash reaction will also occur, which makes the interface interaction between the regenerated sand particles and the slag more intense, strengthens the interface transition zone, and improves the interface bonding strength.

[0023] The recycled bricks of the present invention are originally all from the wastes at the construction site of urban underground transportation projects, including excavation slag, waste concrete and waste slurry, which fully reflects the concept of on-site digestion and in-situ utilization of construction wastes. In particular, the comprehensive utilization rate of excavation slag and recycled aggregate processing waste slurry is extremely low at present. The present invention provides a simple, easy and low-cost new way to utilize the two wastes.

[0024] The composition of recycled bricks is close to that of soil, and no strong alkaline materials such as cement, lime and activators are used. They are more compatible with the surrounding environment and can be used as slope protection paving, ecological retaining walls, etc. They can be returned to the construction site only, saving construction costs. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and beneficial effects of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention. Example 1

[0026] A kind of recycled bricks from wastes in the construction site of a fully underground transportation project comprises: by mass percentage, 50% of excavation debris, 40% of recycled sand from cutting and dismantling temporary supporting concrete beams and columns, and 10% of recycled sand making waste slurry water from cutting and dismantling temporary supporting concrete beams and columns.

[0027] Excavation slag is produced by open or dark excavation of tunnels by tunnel boring machines / shield machines. The produced slag is sieved through a 2mm sieve to remove large particles and then spread on the surface of the open space and naturally dried to a natural moisture content of about 10%; the regenerated sand for temporary support concrete beams and columns is made from concrete blocks cut and removed from temporary support concrete beams and columns on the project site, crushed and recycled steel, and then prepared by wet sand making process to obtain regenerated sand. The moisture content of the regenerated sand after storage is about 5%, and other physical and chemical indicators meet the requirements of Grade 1 distribution area and Class II medium sand specified in GB / T 25176 "Regenerated Fine Aggregates for Concrete and Mortar"; the waste slurry water from the regenerated sand making process of temporary support concrete beams and columns is the sand washing waste slurry water discharged during the process of preparing regenerated sand by wet sand making process after the concrete blocks are cut and removed from temporary support concrete beams and columns on the project site, crushed and recycled steel, and then the waste slurry water is collected in the sump and pumped into the mixing tank by a slurry pump, stirred and concentrated to make the solid content of the waste slurry water reach 20%, and the fineness of solid particles in the waste slurry water ≤0.15 mm, and more than 90% of the solid particles have a fineness of ≤0.075 mm; the concrete strength grade of the temporary supporting concrete beams and columns is C30, and the service life before cutting and demolition is 10 months.

[0028] The method for preparing recycled bricks from waste at the construction site of the fully underground transportation project is:

[0029] Excavation debris, regenerated sand and waste slurry water are measured separately;

[0030] The materials are added into a vacuum clay mixer for mixing and stirring to obtain a mixture;

[0031] The mixed material is input into a spiral extruder for extrusion molding; the extruded block is directly cut online into green billets with a size of 240 mm×115 mm×53 mm.

[0032] Green pieces are stacked and cured in a solar curing room at a temperature of 30-50°C.

[0033] After 7 days of curing, the compressive strength of recycled bricks is 1.63MPa; after 28 days of curing, the compressive strength is 3.91MPa and the flexural strength is 1.62MPa.

[0034] Comparative Example 1

[0035] A kind of recycled bricks from wastes in the construction site of a fully underground transportation project comprises: by mass percentage, 40% of excavation debris, 10% of dry cement powder, 40% of recycled sand from cutting and dismantling temporary supporting concrete beams and columns, and 10% of waste slurry water from recycled sand from cutting and dismantling temporary supporting concrete beams and columns.

[0036] Excavation slag is produced by open or dark excavation of tunnels by tunnel boring machines / shield machines. The produced slag is sieved through a 2mm sieve to remove large particles and then spread on the surface of the open space and naturally dried to a natural moisture content of about 12.5%; the regenerated sand for temporary support concrete beams and columns is made from concrete blocks cut and removed from temporary support concrete beams and columns on the project site, crushed and recycled steel, and then prepared by wet sand making process to obtain regenerated sand. The moisture content of the regenerated sand after storage is about 5%, and other physical and chemical indicators meet the requirements of Grade 1 distribution area and Class II medium sand specified in GB / T 25176 "Regenerated Fine Aggregates for Concrete and Mortar"; the waste slurry water from the regenerated sand making process of temporary support concrete beams and columns is the sand washing waste slurry water discharged during the process of preparing regenerated sand by wet sand making process after the concrete blocks are cut and removed from temporary support concrete beams and columns on the project site, crushed and recycled steel, and then the waste slurry water is collected in the sump and pumped into the mixing tank by a slurry pump, stirred and concentrated to make the solid content of the waste slurry water reach 20%, and the fineness of solid particles in the waste slurry water ≤0.15 mm, and more than 90% of the solid particles have a fineness of ≤0.075 mm; the concrete strength grade of the temporary supporting concrete beams and columns is C30, and the service life before cutting and demolition is 10 months.

[0037] The method for preparing recycled bricks from waste at the construction site of the fully underground transportation project is:

[0038] Excavation debris, regenerated sand and waste slurry water are measured separately;

[0039] The materials are added into a vacuum clay mixer for mixing and stirring to obtain a mixture;

[0040] The mixed material is input into a spiral extruder for extrusion molding; the extruded block is directly cut online into green billets with a size of 240 mm×115 mm×53 mm.

[0041] Green pieces are stacked and cured in a solar curing room at a temperature of 30-50°C.

[0042] Recycled bricks cured for 7 days: compressive strength 1.82MPa; cured for 28 days: compressive strength 4.21MPa, flexural strength 1.02MPa.

[0043] By replacing half of the excavation debris with cement, the compressive strength of the recycled bricks finally produced increased, but the flexural strength was significantly reduced. Example 2

[0044] A kind of recycled bricks from wastes in the construction site of a fully underground transportation project comprises: by mass percentage, 50% of excavation debris, 38% of recycled sand from cutting and dismantling temporary supporting concrete beams and columns, and 12% of recycled sand making waste slurry water from cutting and dismantling temporary supporting concrete beams and columns.

[0045] Excavation slag is produced by open or dark excavation of tunnels by tunnel boring machines / shield machines. The produced slag is sieved through a 2mm sieve to remove large particles and then spread on the surface of the open space and naturally dried to a natural moisture content of about 10%; the regenerated sand for temporary support concrete beams and columns is made from concrete blocks cut and removed from temporary support concrete beams and columns on the project site, crushed and recycled steel, and then prepared by wet sand making process to obtain regenerated sand. The moisture content of the regenerated sand after storage is about 5%, and other physical and chemical indicators meet the requirements of Grade 1 distribution area and Class II medium sand specified in GB / T 25176 "Regenerated Fine Aggregates for Concrete and Mortar"; the waste slurry water from the regenerated sand making process of temporary support concrete beams and columns is the sand washing waste slurry water discharged during the process of preparing regenerated sand by wet sand making process after the concrete blocks are cut and removed from temporary support concrete beams and columns on the project site, crushed and recycled steel, and then the waste slurry water is collected in the sump and pumped into the mixing tank by a slurry pump, stirred and concentrated to make the solid content of the waste slurry water reach 20%, and the fineness of solid particles in the waste slurry water ≤0.15 mm, and more than 90% of the solid particles have a fineness of ≤0.075 mm; the concrete strength grade of the temporary supporting concrete beams and columns is C30, and the service life before cutting and demolition is 10 months.

[0046] The method for preparing recycled bricks from waste at the construction site of the fully underground transportation project is:

[0047] Excavation debris, regenerated sand and waste slurry water are measured separately;

[0048] The materials are added into a vacuum clay mixer for mixing and stirring to obtain a mixture;

[0049] The mixed material is input into a spiral extruder for extrusion molding; the extruded block is directly cut online into green pieces with a size of 240 mm×115 mm×53 mm;

[0050] Green parts are stacked and maintained in solar curing room.

[0051] The compressive strength of recycled bricks is 2.07MPa after 7d of curing, and 4.46MPa after 28d of curing. Example 3

[0052] A fully underground transportation engineering construction site waste recycled brick comprises: by mass percentage, 55% of excavation debris, 32% of recycled sand from cutting and dismantling temporary support concrete beams and columns, and 13% of recycled sand making waste slurry water from cutting and dismantling temporary support concrete beams and columns.

[0053] Excavation slag is produced by open or dark excavation of tunnels by tunnel boring machines / shield machines. The produced slag is sieved through a 2mm sieve to remove large particles and then spread on the surface of the open space and naturally dried to a natural moisture content of about 10%; the regenerated sand for temporary support concrete beams and columns is made from concrete blocks cut and removed from temporary support concrete beams and columns on the project site, crushed and recycled steel, and then prepared by wet sand making process to obtain regenerated sand. The moisture content of the regenerated sand after storage is about 5%, and other physical and chemical indicators meet the requirements of Grade 1 distribution area and Class II medium sand specified in GB / T 25176 "Regenerated Fine Aggregates for Concrete and Mortar"; the waste slurry water from the regenerated sand making process of temporary support concrete beams and columns is the sand washing waste slurry water discharged during the process of preparing regenerated sand by wet sand making process after the concrete blocks are cut and removed from temporary support concrete beams and columns on the project site, crushed and recycled steel, and then the waste slurry water is collected in the sump and pumped into the mixing tank by a slurry pump, stirred and concentrated to make the solid content of the waste slurry water reach 20%, and the fineness of solid particles in the waste slurry water ≤0.15 mm, and more than 90% of the solid particles have a fineness of ≤0.075 mm; the concrete strength grade of the temporary supporting concrete beams and columns is C30, and the service life before cutting and demolition is 6 months.

[0054] The method for preparing recycled bricks from waste at the construction site of the fully underground transportation project is:

[0055] Excavation debris, regenerated sand and waste slurry water are measured separately;

[0056] The materials are added into a vacuum clay mixer for mixing and stirring to obtain a mixture;

[0057] The mixed material is input into a spiral extruder for extrusion molding; the extruded block is directly cut online into green pieces with a size of 240 mm×115 mm×53 mm;

[0058] Green parts are stacked and maintained in solar curing room.

[0059] The compressive strength of recycled bricks is 1.85MPa after 7 days of curing, and 4.15MPa after 28 days of curing. Example 4

[0060] A kind of recycled bricks from wastes in the construction site of a fully underground transportation project comprises: by mass percentage, 55% of excavation debris, 30% of recycled sand from cutting and dismantling temporary supporting concrete beams and columns, and 15% of recycled sand making waste slurry water from cutting and dismantling temporary supporting concrete beams and columns.

[0061] Excavation slag is produced by open or dark excavation of tunnels by tunnel boring machines / shield machines. The produced slag is sieved through a 2mm sieve to remove large particles and then spread on the surface of the open space and naturally dried to a natural moisture content of about 10%; the regenerated sand for temporary support concrete beams and columns is made from concrete blocks cut and removed from temporary support concrete beams and columns on the project site, crushed and recycled steel, and then prepared by wet sand making process to obtain regenerated sand. The moisture content of the regenerated sand after storage is about 5%, and other physical and chemical indicators meet the requirements of Grade 1 distribution area and Class II medium sand specified in GB / T 25176 "Regenerated Fine Aggregates for Concrete and Mortar"; the waste slurry water from the regenerated sand making process of temporary support concrete beams and columns is the sand washing waste slurry water discharged during the process of preparing regenerated sand by wet sand making process after the concrete blocks are cut and removed from temporary support concrete beams and columns on the project site, crushed and recycled steel, and then the waste slurry water is collected in the sump and pumped into the mixing tank by a slurry pump, stirred and concentrated to make the solid content of the waste slurry water reach 20%, and the fineness of solid particles in the waste slurry water ≤0.15 mm, and more than 90% of the solid particles have a fineness of ≤0.075 mm; the concrete strength grade of the temporary supporting concrete beams and columns is C30, and the service life before cutting and dismantling is 2 months.

[0062] The method for preparing recycled bricks from waste at the construction site of the fully underground transportation project is:

[0063] Excavation debris, regenerated sand and waste slurry water are measured separately;

[0064] The materials are added into a vacuum clay mixer for mixing and stirring to obtain a mixture;

[0065] The mixed material is input into a spiral extruder for extrusion molding; the extruded block is directly cut online into green pieces with a size of 240 mm×115 mm×53 mm;

[0066] Green parts are stacked and maintained in solar curing room.

[0067] The compressive strength of recycled bricks is 1.71 MPa after 7 days of curing, and 3.97 MPa after 28 days of curing. Example 5

[0068] A kind of recycled bricks from wastes in the construction site of a fully underground transportation project comprises: by mass percentage, 60% of excavation debris, 30% of recycled sand from cutting and dismantling temporary supporting concrete beams and columns, and 10% of recycled sand making waste slurry water from cutting and dismantling temporary supporting concrete beams and columns.

[0069] Excavation slag is produced by open or dark excavation of tunnels by tunnel boring machines / shield machines. The produced slag is sieved through a 2mm sieve to remove large particles and then spread on the surface of the open space and naturally dried to a natural moisture content of about 10%; the regenerated sand for temporary support concrete beams and columns is made from concrete blocks cut and removed from temporary support concrete beams and columns on the project site, crushed and recycled steel, and then prepared by wet sand making process to obtain regenerated sand. The moisture content of the regenerated sand after storage is about 5%, and other physical and chemical indicators meet the requirements of Grade 1 distribution area and Class II medium sand specified in GB / T 25176 "Regenerated Fine Aggregates for Concrete and Mortar"; the waste slurry water from the regenerated sand making process of temporary support concrete beams and columns is the sand washing waste slurry water discharged during the process of preparing regenerated sand by wet sand making process after the concrete blocks are cut and removed from temporary support concrete beams and columns on the project site, crushed and recycled steel, and then the waste slurry water is collected in the sump and pumped into the mixing tank by a slurry pump, stirred and concentrated to make the solid content of the waste slurry water reach 20%, and the fineness of solid particles in the waste slurry water ≤0.15 mm, and more than 90% of the solid particles have a fineness of ≤0.075 mm; the concrete strength grade of the temporary supporting concrete beams and columns is C30, and the service life before cutting and demolition is 6 months.

[0070] The method for preparing recycled bricks from waste at the construction site of the fully underground transportation project is:

[0071] Excavation debris, regenerated sand and waste slurry water are measured separately;

[0072] The materials are added into a vacuum clay mixer for mixing and stirring to obtain a mixture;

[0073] The mixed material is input into a spiral extruder for extrusion molding; the extruded block is directly cut online into green pieces with a size of 240 mm×115 mm×53 mm;

[0074] Green parts are stacked and maintained in solar curing room.

[0075] The compressive strength of recycled bricks after 7 days of curing is 2.09 MPa, and after 28 days of curing, the compressive strength is 4.64 MPa.

[0076] Comparative Example 5

[0077] A kind of recycled bricks from wastes in the construction site of a fully underground transportation project comprises: by mass percentage, 60% of excavation debris, 30% of recycled sand from cutting and dismantling temporary supporting concrete beams and columns, and 10% of recycled sand making waste slurry water from cutting and dismantling temporary supporting concrete beams and columns.

[0078] Excavation slag is produced by open or dark excavation of tunnels by tunnel boring machines / shield machines. The slag is sieved through a 2mm sieve to remove large particles and then spread on the surface of the open space and naturally dried to a natural moisture content of about 10%; the regenerated sand for temporary support concrete beams and columns is made from concrete blocks cut and removed from temporary support concrete beams and columns on the project site, crushed and recycled steel, and then prepared by wet sand making process to obtain regenerated sand. The moisture content of the regenerated sand after storage is about 5%, and other physical and chemical indicators meet the requirements of Grade 1 distribution area and Class II medium sand specified in GB / T 25176 "Regenerated Fine Aggregates for Concrete and Mortar"; the waste slurry water from the regenerated sand making process of temporary support concrete beams and columns is the sand washing waste slurry water discharged during the process of preparing regenerated sand by wet sand making process after the concrete blocks are cut and removed from temporary support concrete beams and columns on the project site, crushed and recycled steel, and then the waste slurry water is collected in the sump and pumped into the mixing tank by a slurry pump, stirred and concentrated to make the solid content of the waste slurry water reach 10%, and the fineness of solid particles in the waste slurry water is ≤0.15 mm, and more than 90% of the solid particles have a fineness of ≤0.075 mm; the concrete strength grade of the temporary supporting concrete beams and columns is C30, and the service life before cutting and dismantling is 6 months.

[0079] The method for preparing recycled bricks from waste at the construction site of the fully underground transportation project is:

[0080] Excavation debris, regenerated sand and waste slurry water are measured separately;

[0081] The materials are added into a vacuum clay mixer for mixing and stirring to obtain a mixture;

[0082] The mixed material is input into a spiral extruder for extrusion molding; the extruded block is directly cut online into green pieces with a size of 240 mm×115 mm×53 mm;

[0083] Green parts are stacked and maintained in solar curing room.

[0084] The compressive strength of recycled bricks is 1.59 MPa after 7 days of curing, and 3.64 MPa after 28 days of curing.

[0085] In the present invention, the total water content of the mixed material is controlled between 15-17%. When the water content exceeds 19%, the compressive strength of the prepared recycled brick will be significantly reduced. Example 6

[0086] A kind of recycled bricks from wastes in the construction site of a fully underground transportation project comprises: by mass percentage, 60% of excavation debris, 28% of recycled sand from cutting and dismantling temporary supporting concrete beams and columns, and 12% of recycled sand making waste slurry water from cutting and dismantling temporary supporting concrete beams and columns.

[0087] Excavation slag is produced by open or dark excavation of tunnels by tunnel boring machines / shield machines. The produced slag is sieved through a 2mm sieve to remove large particles and then spread on the surface of the open space and naturally dried to a natural moisture content of about 10%; the regenerated sand for temporary support concrete beams and columns is made from concrete blocks cut and removed from temporary support concrete beams and columns on the project site, crushed and recycled steel, and then prepared by wet sand making process to obtain regenerated sand. The moisture content of the regenerated sand after storage is about 5%, and other physical and chemical indicators meet the requirements of Grade 1 distribution area and Class II medium sand specified in GB / T 25176 "Regenerated Fine Aggregates for Concrete and Mortar"; the waste slurry water from the regenerated sand making process of temporary support concrete beams and columns is the sand washing waste slurry water discharged during the process of preparing regenerated sand by wet sand making process after the concrete blocks are cut and removed from temporary support concrete beams and columns on the project site, crushed and recycled steel, and then the waste slurry water is collected in the sump and pumped into the mixing tank by a slurry pump, stirred and concentrated to make the solid content of the waste slurry water reach 15%, and the fineness of solid particles in the waste slurry water ≤0.15 mm, and more than 90% of the solid particles have a fineness of ≤0.075 mm; the concrete strength grade of the temporary supporting concrete beams and columns is C30, and the service life before cutting and demolition is 8 months.

[0088] The method for preparing recycled bricks from waste at the construction site of the fully underground transportation project is:

[0089] Excavation debris, regenerated sand and waste slurry water are measured separately;

[0090] The materials are added into a vacuum clay mixer for mixing and stirring to obtain a mixture;

[0091] The mixed material is input into a spiral extruder for extrusion molding; the extruded block is directly cut online into green pieces with a size of 240 mm×115 mm×53 mm;

[0092] Green parts are stacked and maintained in solar curing room.

[0093] The compressive strength of recycled bricks after 7 days of curing is 2.22 MPa, and the compressive strength after 28 days of curing is 4.82 MPa.

[0094] In summary, the present invention provides a simple, practical, economical and feasible way for the treatment and disposal of waste at the construction site of urban underground transportation projects, and realizes the productization and high-efficiency, low-cost preparation and application of waste.

[0095] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.

Claims

1. A fully underground transportation engineering construction site waste recycled brick, characterized in that: The raw materials for preparing the recycled bricks are composed of 50%-60wt% of excavation debris, 28%-40wt% of recycled sand from cutting and dismantling temporary support concrete beams and columns, and 8%-15wt% of recycled sand waste slurry water from cutting and dismantling temporary support concrete beams and columns; the excavation debris is produced by open or dark excavation of tunnels by tunnel boring machines / shield machines, the particle size of the excavation debris is less than 2mm, and the moisture content is 8-12wt%; the concrete of the temporary support concrete beams and columns has a service life of ≤1 year before cutting and dismantling; The temporary supporting concrete beam and column regenerated sand making waste slurry water is the sand washing waste slurry water discharged in the process of preparing regenerated sand by wet sand making process after the temporary supporting concrete beam and column on the project site is cut and dismantled concrete blocks, crushed and steel is recycled. The waste slurry water enters the collection tank for collection, and is pumped into the mixing tank by a mud pump, stirred and concentrated to make the solid content of the waste slurry water reach 10-20%, the fineness of solid particles in the waste slurry water is ≤0.15 mm, and more than 90% of the solid particles are ≤0.075 mm.

2. The fully underground transportation engineering construction site waste recycled brick according to claim 1, characterized in that: The temporary support concrete beam and column regenerated sand is made from concrete blocks cut and removed from temporary support concrete beams and columns on the construction site, crushed and recycled steel, and then prepared by a wet sand making process. The moisture content of the regenerated sand is 4-6%, and the physical and chemical indicators meet the requirements of Grade 1 distribution area and Class II medium sand specified in GB / T 25176 "Regenerated Fine Aggregate for Concrete and Mortar".

3. The method for preparing the recycled bricks from wastes in the construction site of the fully underground transportation project according to claim 1 or 2, characterized in that: The following steps are involved: S1 Excavation waste soil, cut and dismantle temporary support concrete beam and column regenerated sand and cut and dismantle temporary support concrete beam and column regenerated sand sand making waste slurry water are measured separately; S2 Add the materials into a vacuum clay mixer and mix them to obtain a mixture; S3 mixed material is input into the screw extruder for extrusion molding; S4 extrusion blocks are directly cut into green pieces online; S5 green bricks are stacked and cured in a solar curing room, thus preparing recycled bricks from waste at the construction site of the fully underground transportation project.

4. The preparation method according to claim 3, characterized in that: The curing temperature of step S5 is 30-50 degrees Celsius, and the curing time is greater than 28 days.

Citation Information

Patent Citations

  • Self-compacting concrete prepared from concrete mixing station waste slurry

    CN105776994A

  • Salt frost resistant concrete curbstone prepared from waste slurry of concrete mixing station and preparation method thereof

    CN105819783A

  • Alkali-activated waste residue firing-free brick and preparation method thereof

    CN111072329A

  • Single-component regenerated geopolymer cement concrete

    CN111548068A

  • Engineering residue soil baking-free brick and preparation method thereof

    CN115321893A