A polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel and its preparation method and application

Through the three-dimensional porous structure of polyacrylonitrile/MXene@Ag-Ag2S nanofiber aerogel and the photothermal conversion performance of Ag-Ag2S nanoparticles, the problem of organic dye pollution is solved, and high-efficiency and low-cost photocatalytic degradation is achieved. Effective, suitable for sewage treatment.

CN116515227BActive Publication Date: 2024-11-08SUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310290176.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-11-08
Estimated Expiration
2043-03-23

AI Technical Summary

Technical Problem

The prior art is difficult to effectively deal with organic dye pollution, the traditional methods are complex and costly, the semiconductor photocatalysts have poor response to ultraviolet light, and the existing hydrogel materials lack three-dimensional shape and mechanical properties, and the degradation efficiency is low.

Method used

Polyacrylonitrile/MXene@Ag-Ag2S nanofiber aerogel is used to form a three-dimensional porous structure through hydrogen bonding. The photothermal conversion performance of Ag-Ag2S nanoparticles and MXene is used to achieve continuous photodegradation of organic dyes.

Benefits of technology

It has achieved efficient photocatalytic degradation of organic dyes, with a degradation rate of more than 90%, a porosity of up to 97.5%. The material can be recycled and is suitable for a wide range of wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116515227B_ABST
    Figure CN116515227B_ABST
Patent Text Reader

Abstract

The present invention relates to a polyacrylonitrile / MXene@Ag‑Ag2S nanofiber aerogel and a preparation method and application thereof, and belongs to the technical field of water purification materials. The nanofiber aerogel is composed of alkaline-decomposed polyacrylonitrile fibers, MXene, and Ag‑Ag2S nanoparticles loaded on MXene, and has a porous and high specific surface area. The present invention combines the respective characteristics of MXene materials and photocatalytic semiconductor materials, silver sulfide, to photodegrade organic dyes such as methylene blue and rhodamine 6G in water bodies under visible light illumination conditions to achieve the purpose of purifying water, and the photocatalytic degradation rate reaches more than 90%, wherein the maximum degradation rate of methylene blue reaches 98.85%, and the maximum degradation rate of rhodamine 6G reaches 95.67%. It has many advantages such as fast degradation speed, high efficiency, low energy consumption, good universality, etc. The aerogel can also be recycled and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of water purification materials, and in particular to a polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel and a preparation method and application thereof. Background Art

[0002] While industrial development brings convenience to people's lives, it also brings people many environmental pollution problems that cannot be ignored. Among them, water pollution caused by organic dyes is the most serious. According to statistics, there are already 100,000 kinds of dyes used in commerce. In China, the annual output of dyes has reached nearly 150,000 tons. During the use of these dyes, 10% to 15% of the dyes are discharged into the water, and most organic dyes have extremely high biological toxicity and carcinogenicity, such as rhodamine and methylene blue. Most dyes are difficult to be biodegraded due to their large molecular weight and complex structure, which will cause serious damage to the ecological balance in the water, and water resources are facing great threats. It also has a great impact on human health. Therefore, the degradation of dye wastewater has become a water pollution problem that needs to be solved urgently.

[0003] How to effectively treat organic dyes is the focus of research, and the main methods used include chemical precipitation, redox, electrochemical technology and ion exchange. These traditional methods are limited in practical application due to their complex process operation and high cost. However, the semiconductor photocatalytic degradation method uses photocatalysts to generate a series of holes and free radicals with strong oxidation ability under light conditions, and further oxidative decomposition reactions occur to degrade organic pollutants into inorganic substances such as CO2 and H2O, thereby achieving a thorough oxidation and decomposition of organic matter. It has many advantages such as simple operation, high efficiency, low energy consumption, and good universality. The most important thing is that there is no secondary pollution and it can be recycled. However, the currently used semiconductor photocatalysts such as TiO2 are only photoresponsive to ultraviolet light.

[0004] As a precious metal nanomaterial, Ag plays an important role in catalysis, optics and surface enhanced Raman. As precious metal silver has a large number of free electrons and its own low resistance, it is easy to produce surface plasmon resonance effect and show significant photothermal conversion characteristics. At the same time, Ag2S, as a narrow-bandgap semiconductor photocatalyst, has a bandgap width of 1.0eV and has good photoelectric, thermoelectric, light absorption and photocatalytic properties. Because it can effectively absorb light energy, it is widely used in the photocatalytic degradation of organic dyes and harmful pollutants.

[0005] However, the band gap of pure semiconductor nanomaterial Ag2S limits the wavelength range of light it can absorb, thus affecting the application of semiconductor nanomaterials in light-to-heat conversion. Therefore, through doping, semiconductor nanomaterials can produce sub-band gap defect states, effectively narrowing the band gap, thereby expanding the range of wavelengths absorbed by semiconductor nanomaterials, absorbing wavelengths in the visible light range, and alleviating the constraints of semiconductor nanomaterials on the wavelength range of light absorption. Therefore, the advantages of Ag2S and Ag are combined to prepare metal-semiconductor composite nanoparticles Ag-Ag2S, which have ultraviolet, visible and near-infrared light absorption properties, and as a photocatalyst, it embodies excellent light-to-heat conversion characteristics and photocatalytic degradation of organic matter.

[0006] MXene materials are a type of metal carbon / nitride with a two-dimensional layered structure. MXene materials are widely used in energy storage, catalysis, sensors, composite material reinforcement, sewage treatment and other fields due to their high specific surface area, high electrical conductivity, good hydrophilicity, rich surface chemical groups and active sites, and excellent photothermal conversion performance. Among them, composites based on MXene and semiconductor materials are widely used in the field of photocatalysis. Since MXene can promote the separation of electrons and holes in semiconductors, composites are often more efficient than pure semiconductor materials; and three-dimensional semiconductor gel composites with polymers and MXene as skeletons have higher specific surface areas and can provide more sites for reactions. While accelerating the reaction rate, the composites also have excellent adsorption properties; in addition, the three-dimensional structure makes the removal and recycling of the composites more convenient and feasible.

[0007] The Chinese invention patent application with publication number CN108816247 B discloses a method for photodegrading organic dyes using silver sulfide quantum dots-graphene hydrogels. The invention combines silver sulfide quantum dots with graphene materials and utilizes the silver sulfide quantum dots to photocatalytically degrade organic dyes by using the quantum size effect. However, the hydrogel prepared by the above method cannot meet certain requirements for the three-dimensional shape or mechanical properties of the material because it does not have a polymer as a skeleton and support, and the degradation efficiency is relatively low.

[0008] The Chinese invention patent with application number 202010908333.X reports a method for preparing a photocatalytically functional magnetic graphene-based aerogel. First, the photocatalytic material tetraaminotitanium cyanine iron is prepared, and then the magnetic graphene-based aerogel is prepared by loading magnetic particles on the graphene substrate. Finally, the tetraaminotitanium cyanine iron is grafted to the surface of the magnetic graphene-based aerogel by amidation reaction to obtain a photocatalytically functional magnetic graphene-based aerogel material. The material has an integrated adsorption-degradation effect and a physical magnetic separation function, and can be widely used in the adsorption and degradation of benzo-α-pyrene (BaP)-containing contaminated systems. However, the sensitivity of the aerogel to dyes and the range of choices for adsorption and degradation are relatively limited, and it is easy to cause secondary pollution.

[0009] Therefore, developing a method for photocatalytic degradation of organic pollutants using polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel that can be used for continuous photodegradation of dyes is a technical problem that needs to be solved urgently in this field, and no public reports have been seen yet. Summary of the invention

[0010] In order to solve the above technical problems, the present invention provides a polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel and its preparation method and application. Since Ag2S nanoparticles have a large light absorption coefficient, good photoelectric properties, and are green and non-toxic, they are a good organic dye catalytic degradation medium, combined with the two-dimensional material MXene with advantages such as good hydrophilicity, high specific surface area, abundant active sites and excellent photothermal conversion performance. At the same time, the surface of the alkaline-hydrolyzed polyacrylonitrile fiber contains abundant carboxyl groups, which can form dense hydrogen bonds with a large number of hydroxyl groups on the surface of MXene to obtain a nanofiber aerogel with a certain strength, thereby realizing the continuous photodegradation of organic dyes.

[0011] The present invention is achieved through the following technical solutions:

[0012] The first object of the present invention is to provide a polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel, wherein the polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel is composed of polyacrylonitrile nanofibers, MXene, and Ag-Ag2S nanoparticles loaded on MXene; the polyacrylonitrile nanofibers are bonded to MXene through hydrogen bonds; the polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel is a three-dimensional porous structure with a density of 20 mg / cm 3 ~50mg / cm 3 , the porosity is 94.2%~97.5%.

[0013] In one embodiment of the present invention, the diameter of the Ag-Ag2S nanoparticles is 10 nm to 500 nm.

[0014] The second object of the present invention is to provide a method for preparing polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel, comprising the following steps:

[0015] (1) MXene powder is dissolved in water, and the precipitate obtained after centrifugation is dispersed in water through ultrasound, repeated oscillation and centrifugation to obtain a flaky MXene dispersion; the centrifugal speed is 3000 rpm to 5000 rpm, the centrifugal washing time is 5 min to 10 min each time, and the number of centrifugation is 7 to 8 times; wherein, repeated oscillation and centrifugation are for better exfoliation and stratification of MXene;

[0016] (2) adding silver nitrate, thiourea and alkali to the flaked MXene dispersion obtained in step (1), mixing and reacting under light conditions to obtain a MXene@Ag-Ag2S dispersion;

[0017] (3) Mixing the alkaline hydrolyzed polyacrylonitrile nanofibers with the MXene@Ag-Ag2S dispersion obtained in step (2) to obtain the polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel.

[0018] In one embodiment of the present invention, in step (2), the illumination time is 3h to 5h.

[0019] In one embodiment of the present invention, in step (2), the mass ratio of the silver nitrate, thiourea and alkali is 2-4:1:1.

[0020] In one embodiment of the present invention, in step (3), the mass ratio of the alkaline hydrolyzed polyacrylonitrile nanofibers to the MXene@Ag-Ag2S dispersion is 1 to 2:1.

[0021] In one embodiment of the present invention, in step (3), the alkaline hydrolyzed polyacrylonitrile nanofibers are prepared by the following method:

[0022] S1, heating and dissolving polyacrylonitrile in an organic solvent to obtain a polyacrylonitrile spinning solution, and preparing a polyacrylonitrile nanofiber membrane by electrospinning; cutting the polyacrylonitrile nanofiber membrane into pieces, and homogenizing it in water to obtain a polyacrylonitrile nanofiber dispersion;

[0023] S2, adding the polyacrylonitrile nanofiber dispersion obtained in step S1 into an alkaline solution for heating and alkaline hydrolysis for 20 minutes to 30 minutes to obtain alkaline-hydrolyzed polyacrylonitrile nanofibers.

[0024] In one embodiment of the present invention, the alkaline hydrolyzed polyacrylonitrile (PAN) nanofibers are prepared by the following method:

[0025] Take polyacrylonitrile and N, N-dimethylformamide (DMF) solution (PAN solution concentration is 12wt%) and stir magnetically in an oil bath pot at a speed of 500rpm-800rpm; then prepare polyacrylonitrile nanofiber membrane by electrostatic spinning (spinning voltage is 7.9kV-12kV, liquid flow rate is 0.4mL / h-0.8mL / h, and the distance between the syringe port and the roller receiving device is 16cm); cut the polyacrylonitrile nanofiber membrane into pieces, take the polyacrylonitrile fiber membrane and disperse it in pure water, and use a high-speed stirrer to break up the homogenized polyacrylonitrile nanofiber blocks to obtain a water dispersion of polyacrylonitrile nanofiber. Finally, take ethanol, ultrapure water and NaOH and stir magnetically in an oil bath pot at 85℃ until the solution boils, add the polyacrylonitrile nanofiber dispersion, and alkaline hydrolyze for 20min-30min, then put it in a centrifuge for centrifugal washing for 3-5 times, remove the excess alkaline solution, and obtain the polyacrylonitrile nanofiber after alkaline hydrolysis.

[0026] The third object of the present invention is to provide the application of the polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel in degrading dyes.

[0027] In one embodiment of the present invention, the concentration of the dye is 1 mg / L-10 mg / L.

[0028] In one embodiment of the present invention, the application method is: mixing polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel with a dye and catalytically degrading it under light conditions.

[0029] The polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel of the present invention has extremely low density, large specific surface area and adjustable pore structure, making it an ideal adsorption material. The super-wettable aerogel material is combined with the MXene material having excellent conductivity, hydrophilicity, rich surface functional group chemical properties and adjustable layered structure, and the photocatalyst material Ag-Ag2S having both strong photocatalytic activity and strong adsorption performance, providing a more effective approach to sewage treatment fields such as photodegradation of organic dyes.

[0030] The above technical solution of the present invention has the following advantages compared with the prior art:

[0031] (1) The surface of alkaline hydrolyzed polyacrylonitrile fiber contains a large number of carboxyl and amide groups, which can make the hydroxyl groups on the surface of MXene combine to form hydrogen bonds. The prepared aerogel is easy to shape and has good strength and elasticity. The MXene@Ag-Ag2S aerogel without the addition of PAN nanofibers has low strength and cannot meet some requirements for the three-dimensional shape or mechanical properties of the material, and it is easy to fall apart. The nanofiber aerogel has a high specific surface area and super hydrophilicity, with a porosity of up to 97.5%.

[0032] (2) In a single-layer or few-layer MXene nanosheet, Ag-Ag2S nanoparticles are generated in situ on the MXene surface by ultraviolet light, and the particles and MXene are tightly bound and evenly dispersed. Compared with PAN / MXene nanofiber aerogel, the present invention introduces metal-semiconductor composite nanoparticles Ag-Ag2S with excellent photodegradation performance to combine it with two-dimensional material MXene with rich surface active sites and excellent photothermal conversion performance, thereby greatly improving the surface utilization rate and photocatalytic active sites of the material, thereby improving the photodegradation performance of the material. Pure MXene is easy to self-stack, resulting in a decrease in specific surface area and porosity. Using alkaline hydrolysis of PAN nanofibers to intercalate and support MXene can effectively increase the specific surface area and porosity, increase active sites, and improve photodegradation performance.

[0033] (3) The present invention combines the respective characteristics of MXene materials and metal-semiconductor composite nanoparticles Ag-Ag2S with excellent photocatalytic properties, and utilizes the micro-nano-level layered porous structure inside the aerogel and the increased surface roughness caused by the modification of silver-silver sulfide nanoparticles, so as to have a good adsorption capacity for organic dyes. In addition, the aerogel further undergoes an oxidative decomposition reaction under visible light conditions to degrade organic dyes such as methylene blue and rhodamine 6G into inorganic substances such as CO2 and H2O, thereby achieving the purpose of thorough oxidative decomposition of organic dyes and purification of water. The photocatalytic degradation rate is more than 90%, among which the highest degradation rate of methylene blue is 98.85%, and the highest degradation rate of rhodamine 6G is 95.67%.

[0034] (4) The shape of the nanofiber aerogel is controllable and can be prepared into a long column shape for continuous photodegradation of dyes. It has many advantages such as fast degradation rate, high efficiency, low energy consumption, and good universality. The aerogel can also be recycled and has broad application prospects.

[0035] (5) The PAN / MXene@Ag-Ag2S aerogel in the present invention has a strong adsorption capacity for dyes such as methylene blue because the surface of MXene-Ti3C2 is negatively charged and has a good electrostatic interaction with cationic dye molecules. In addition, since MXene and Ag2S are both good photothermal conversion materials, they have a wide spectrum absorption of sunlight. The PAN / MXene@Ag-Ag2S aerogel in the present invention has a wide spectrum universality for the photocatalytic degradation of dyes. Under sunlight conditions, when the concentration of organic dyes methylene blue and rhodamine 6G is 1mg / L-10mg / L, the dye solution can be degraded into a colorless and transparent liquid in just 1 hour, and the photocatalytic degradation rate reaches more than 90%, among which the highest degradation rate of methylene blue reaches 98.85%, and the highest degradation rate of rhodamine 6G reaches 95.67%. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein

[0037] Figure 1 This is a physical picture of the polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel prepared in Example 1 of the present invention, with adjustable length;

[0038] Figure 2 This is a scanning electron microscope photograph of the polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel in Example 1 of the present invention;

[0039] Figure 3 This is a scanning electron microscope photograph of the MXene@Ag-Ag2S solution in Example 1 of the present invention;

[0040] Figure 4 The XRD spectrum of the MXene@Ag-Ag2S solution in Example 1 of the present invention;

[0041] Figure 5 This is the elemental analysis diagram of the polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel in Example 1 of the present invention;

[0042] Figure 6 This is a physical picture of the polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel prepared in Example 2 of the present invention;

[0043] Figure 7 This is a physical picture of the polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel prepared in Example 3 of the present invention;

[0044] Figure 8 A physical picture of the polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel prepared in Example 4 of the present invention (left) and a comparison picture of the aerogel in Example 1;

[0045] Fig. 9 This is a physical picture of the MXene@Ag-Ag2S nanofiber aerogel in Comparative Example 1 of the present invention;

[0046] Fig.10 A diagram of a device for photodegradation in the performance test of the present invention;

[0047] Fig.11 The spectrum of the Rhodamine 6G dye before and after degradation at a concentration of 10 mg / L in the performance test of the present invention;

[0048] Fig.12 The spectrum of the Rhodamine 6G dye before and after degradation at a concentration of 1 mg / L in the performance test of the present invention;

[0049] Fig.13 This is a spectrum diagram of methylene blue dye before and after degradation at a concentration of 10 mg / L in the performance test of the present invention;

[0050] Fig.14 This is a spectrum diagram of methylene blue dye before and after degradation at a concentration of 1 mg / L in the performance test of the present invention;

[0051] Fig.15 This is a photodegradation rate diagram of polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel prepared in Example 1 of the present invention after cyclic degradation;

[0052] Fig.16 This is a spectrum diagram of the polyacrylonitrile / MXene nanofiber aerogel prepared in Comparative Example 2 of the present invention before and after the degradation of methylene blue dye;

[0053] Fig.17 This is a spectrum of the polyacrylonitrile / MXene nanofiber aerogel prepared in Comparative Example 2 of the present invention before and after degradation of Rhodamine 6G dye. DETAILED DESCRIPTION

[0054] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0055] Example 1

[0056] This embodiment provides a method for preparing polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel, and the specific preparation method is as follows:

[0057] (1) Preparation of PAN nanofibers: 1.2 g PAN (polyacrylonitrile) and 8.8 mL N,N-dimethylformamide (DMF) solution were magnetically stirred in an oil bath at 45°C for 4 h to obtain a spinning solution. The spinning solution was then electrospun to obtain a PAN nanofiber membrane (where the spinning voltage was 7.9 kV, the liquid flow rate was 0.4 mL / h, and the distance between the syringe port and the roller receiving device was 16 cm); the polyacrylonitrile nanofiber membrane was cut into pieces, 1 g of the cut PAN fiber membrane was dispersed in 100 mL of pure water, and the homogenized polyacrylonitrile nanofiber blocks were broken up with a high-speed mixer to obtain a water dispersion of polyacrylonitrile nanofibers. Finally, 27 mL of ethanol, 4 mL of ultrapure water and 1.5 g of NaOH were magnetically stirred in an oil bath at 85°C until the solution boiled, and the PAN nanofiber dispersion was added, and alkaline hydrolysis was performed for 30 min, followed by centrifugation and washing for 3 times to remove excess alkaline solution; alkaline hydrolyzed polyacrylonitrile nanofibers were obtained.

[0058] (2) Preparation of MXene@Ag-Ag2S solution: 0.1 g of clay-like MXene powder was added to 10 mL of ultrapure water, ultrasonicated for 3 h (power 90 W), repeatedly oscillated, and then centrifuged at 3000 rpm for 5 min, 7 times. The precipitate after centrifugation was dispersed in water to obtain a flaky MXene dispersion. 0.1 g of silver nitrate, 0.05 g of thiourea and 0.05 g of sodium hydroxide (mass ratio of 2:1:1) were added to the obtained flaky MXene dispersion and magnetically stirred for 4 h. At the same time, ultraviolet light was applied to obtain a MXene solution with in situ grown Ag-Ag2S particles.

[0059] (3) Preparation of PAN / MXene@Ag-Ag2S nanofiber aerogel: The alkaline hydrolyzed PAN short nanofibers were mixed with the MXene@Ag-Ag2S solution in a mass ratio of 1:1, and then placed in a vacuum freeze dryer for freeze drying. The freeze drying temperature was below -50 °C, the pressure was below 20 Pa, and the drying time was 48 h to obtain PAN / MXene@Ag-Ag2S nanofiber aerogel.

[0060] The actual picture of the nanofiber aerogel is as follows Figure 1 As shown; the scanning electron microscope image of polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel is shown Figure 2 As shown; the scanning electron microscope photo of MXene@Ag-Ag2S solution is shown Figure 3 As shown; the XRD spectrum of MXene@Ag-Ag2S solution is as follows Figure 4 As shown; the elemental analysis of polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel is shown Figure 5 shown by Figure 1 to Figure 5 It can be seen that polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel is a three-dimensional porous structure composed of alkaline-hydrolyzed polyacrylonitrile fibers, MXene and Ag-Ag2S nanoparticles loaded on MXene, and Ag-Ag2S is uniformly loaded on MXene, with extremely low density and high porosity.

[0061] Example 2

[0062] This embodiment provides a method for preparing polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel, and the specific preparation method is as follows:

[0063] (1) Preparation of PAN nanofibers: 1.2 g PAN (polyacrylonitrile) and 8.8 mL N,N-dimethylformamide (DMF) solution were magnetically stirred in an oil bath at 45°C for 4 h to obtain a spinning solution. The spinning solution was then electrospun to obtain a PAN nanofiber membrane (spinning voltage was 7.9 kV, liquid flow rate was 0.4 mL / h, and the distance between the syringe port and the roller receiving device was 16 cm); the polyacrylonitrile nanofiber membrane was cut into pieces, 1 g PAN fiber membrane was dispersed in 100 mL pure water, and the polyacrylonitrile nanofiber blocks were broken up and homogenized with a high-speed mixer to obtain a water dispersion of polyacrylonitrile nanofibers. Finally, 27 mL of ethanol, 4 mL of ultrapure water and 1.5 g of NaOH were magnetically stirred in an oil bath at 85°C until the solution boiled, and the PAN nanofiber dispersion was added, and alkaline hydrolysis was performed for 30 min, followed by centrifugation and washing for 3 times to remove excess alkaline solution; alkaline hydrolyzed polyacrylonitrile nanofibers were obtained.

[0064] (2) Preparation of MXene@Ag-Ag2S solution: 0.1 g of clay-like MXene powder was added to 10 mL of ultrapure water, ultrasonicated for 3 h (power 90 W), repeatedly oscillated, and then centrifuged at 3000 rpm for 5 min, 7 times. The precipitate after centrifugation was dispersed in water to obtain a flaky MXene dispersion; 0.15 g of silver nitrate, 0.05 g of thiourea and 0.05 g of sodium hydroxide (mass ratio of 3:1:1) were added to the obtained flaky MXene dispersion and magnetically stirred for 4 h. At the same time, ultraviolet light was applied to obtain a MXene solution with in situ grown Ag-Ag2S particles.

[0065] (3) Preparation of PAN / MXene@Ag-Ag2S nanofiber aerogel: The alkaline hydrolyzed PAN short nanofibers were mixed with the MXene@Ag-Ag2S solution at a mass ratio of 1:1, and then placed in a vacuum freeze dryer for freeze drying. The freeze drying temperature was below -50 °C, the pressure was below 20 Pa, and the drying time was 48 h. The physical picture of the obtained PAN / MXene@Ag-Ag2S nanofiber aerogel is shown in the figure below. Figure 6 shown.

[0066] Example 3

[0067] This embodiment provides a method for preparing polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel, and the specific preparation method is as follows:

[0068] (1) Preparation of PAN nanofibers: 1.2 g PAN (polyacrylonitrile) and 8.8 mL N,N-dimethylformamide (DMF) solution were magnetically stirred in an oil bath at 45°C for 4 h to obtain a spinning solution. The prepared spinning solution was then electrospun to obtain a PAN nanofiber membrane (spinning voltage was 7.9 kV, liquid flow rate was 0.4 mL / h, and the distance between the syringe port and the roller receiving device was 16 cm); the polyacrylonitrile nanofiber membrane was cut into pieces, 1 g PAN fiber membrane was dispersed in 100 mL pure water, and the polyacrylonitrile nanofiber blocks were broken up and homogenized with a high-speed mixer to obtain a water dispersion of polyacrylonitrile nanofibers. Finally, 27 mL of ethanol, 4 mL of ultrapure water and 1.5 g of NaOH were magnetically stirred in an oil bath at 85°C until the solution boiled, and the PAN nanofiber dispersion was added, and alkaline hydrolysis was performed for 30 min, followed by centrifugation and washing for 3 times to remove excess alkaline solution; alkaline hydrolyzed polyacrylonitrile nanofibers were obtained.

[0069] (2) Preparation of MXene@Ag-Ag2S solution: 0.1 g of clay-like MXene powder was added to 10 mL of ultrapure water, ultrasonicated for 3 h (power 90 W), repeatedly oscillated, and then centrifuged at 3000 rpm for 5 min, 7 times. The precipitate after centrifugation was dispersed in water to obtain a flaky MXene dispersion; 0.2 g of silver nitrate, 0.05 g of thiourea and 0.05 g of sodium hydroxide (mass ratio of 4:1:1) were added to the obtained flaky MXene dispersion and magnetically stirred for 4 h. At the same time, ultraviolet light was applied to obtain a MXene solution with in situ grown Ag-Ag2S particles.

[0070] (3) Preparation of PAN / MXene@Ag-Ag2S nanofiber aerogel: The alkaline hydrolyzed PAN short nanofibers were mixed with the MXene@Ag-Ag2S solution at a mass ratio of 1:1, and then placed in a vacuum freeze dryer for freeze drying. The freeze drying temperature was below -50 °C, the pressure was below 20 Pa, and the drying time was 48 h. The physical picture of the obtained PAN / MXene@Ag-Ag2S nanofiber aerogel is shown in the figure below. Figure 7 Place.

[0071] Example 4

[0072] This embodiment provides a method for preparing polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel, and the specific preparation method is as follows:

[0073] (1) Preparation of PAN nanofibers: 1.2 g PAN (polyacrylonitrile) and 8.8 mL N,N-dimethylformamide (DMF) solution were magnetically stirred in an oil bath at 45°C for 4 h to obtain a spinning solution. The prepared spinning solution was then electrospun to obtain a PAN nanofiber membrane (spinning voltage 7.9 kV, liquid flow rate 0.4 mL / h, and the distance between the syringe port and the roller receiving device was 16 cm); the polyacrylonitrile nanofiber membrane was cut into pieces, 1 g PAN fiber membrane was dispersed in 100 mL pure water, and the polyacrylonitrile nanofiber blocks were broken up and homogenized with a high-speed mixer to obtain a water dispersion of polyacrylonitrile nanofibers. Finally, 27 mL of ethanol, 4 mL of ultrapure water and 1.5 g of NaOH were magnetically stirred in an oil bath at 85°C until the solution boiled, and the PAN nanofiber dispersion was added, and alkaline hydrolysis was performed for 30 min, followed by centrifugation and washing for 3 times to remove excess alkaline solution; alkaline hydrolyzed polyacrylonitrile nanofibers were obtained.

[0074] (2) Preparation of MXene@Ag-Ag2S solution: 0.1 g of clay-like MXene powder was added to 10 mL of ultrapure water, ultrasonicated for 3 h (power 90 W), repeatedly oscillated, and then centrifuged at 3000 rpm for 5 min, 7 times. The precipitate after centrifugation was dispersed in water to obtain a flaky MXene dispersion; 0.1 g of silver nitrate, 0.05 g of thiourea and 0.05 g of sodium hydroxide (mass ratio of 2:1:1) were added to the obtained flaky MXene dispersion and magnetically stirred for 4 h. At the same time, ultraviolet light was applied to obtain a MXene solution with in situ grown Ag-Ag2S particles.

[0075] (3) Preparation of PAN / MXene@Ag-Ag2S nanofiber aerogel: The alkaline hydrolyzed PAN short nanofibers and MXene@Ag-Ag2S solution were mixed in a mass ratio of 1:2, and then placed in a vacuum freeze dryer for freeze drying. The freeze drying temperature was below -50 °C, the pressure was below 20 Pa, and the drying time was 48 h to obtain PAN / MXene@Ag-Ag2S nanofiber aerogel.

[0076] The actual picture of the polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel prepared in this example (left) is compared with the aerogel in Example 1. Figure 8 shown.

[0077] In summary, it can be seen that the length of PAN / MXene@Ag-Ag2S nanofiber aerogel can be adjusted by increasing the amount of PAN and MXene@Ag-Ag2S year on year.

[0078] Comparative Example 1

[0079] This comparative example provides a method for preparing an aerogel, and the specific preparation method is as follows:

[0080] (1) Preparation of MXene@Ag-Ag2S solution: 0.1 g of clay-like MXene powder was added to 10 mL of ultrapure water, ultrasonicated for 3 h (power 90 W), repeatedly oscillated, and then centrifuged at 3000 rpm for 5 min, 7 times, and the precipitate after centrifugation was dispersed in water to obtain a flaky MXene dispersion; 0.1 g of silver nitrate, 0.05 g of thiourea and 0.05 g of sodium hydroxide (mass ratio of 2:1:1) were added to the obtained flaky MXene dispersion and magnetically stirred for 4 h, and ultraviolet light was applied at the same time to obtain a MXene solution with in situ growth of Ag-Ag2S particles;

[0081] (2) Preparation of MXene@Ag-Ag2S nanofiber aerogel: The solution was placed in a vacuum freeze dryer for freeze drying at a temperature below -50°C, a pressure below 20 Pa, and a drying time of 48 h to obtain MXene@Ag-Ag2S nanofiber powder. The actual figure is shown in Fig. 9 As shown, it cannot be formed.

[0082] It can be seen that the MXene@Ag-Ag2S aerogel without the addition of PAN nanofibers is more likely to fall apart than the PAN / MXene@Ag-Ag2S aerogel with the addition of PAN nanofibers, has lower strength, and cannot meet the requirements for the three-dimensional shape or mechanical properties of the material.

[0083] Comparative Example 2

[0084] This comparative example provides a method for preparing an aerogel, and the specific preparation method is as follows:

[0085] (1) Preparation of PAN nanofibers: 1.2 g PAN (polyacrylonitrile) and 8.8 mL N,N-dimethylformamide (DMF) solution were magnetically stirred in an oil bath at 45°C for 4 h to obtain a spinning solution. The spinning solution was then electrospun to obtain a PAN nanofiber membrane (where the spinning voltage was 7.9 kV, the liquid flow rate was 0.4 mL / h, and the distance between the syringe port and the roller receiving device was 16 cm); the polyacrylonitrile nanofiber membrane was cut into pieces, 1 g of the cut PAN fiber membrane was dispersed in 100 mL of pure water, and the homogenized polyacrylonitrile nanofiber blocks were broken up with a high-speed mixer to obtain a water dispersion of polyacrylonitrile nanofibers. Finally, 27 mL of ethanol, 4 mL of ultrapure water and 1.5 g of NaOH were magnetically stirred in an oil bath at 85°C until the solution boiled, and the PAN nanofiber dispersion was added, and alkaline hydrolysis was performed for 30 min, followed by centrifugation and washing for 3 times to remove excess alkaline solution; alkaline hydrolyzed polyacrylonitrile nanofibers were obtained.

[0086] (2) Preparation of MXene dispersion: 0.1 g of clay-like MXene powder was added to 10 mL of ultrapure water, and ultrasonicated for 3 hours (power 90 W), repeatedly shaken, and then centrifuged at 3000 rpm for 5 minutes, the number of centrifugations was 7 times, and the precipitate after centrifugation was dispersed in water to obtain a flaky MXene dispersion;

[0087] (3) Preparation of PAN / MXene nanofiber aerogel: Alkaline hydrolyzed PAN nanofibers were mixed with MXene solution in a mass ratio of 1:1, and then placed in a vacuum freeze dryer for freeze drying at a freeze drying temperature below -50°C, a pressure below 20 Pa, and a drying time of 48 h to obtain PAN / MXene nanofiber aerogel.

[0088] It can be seen that PAN / MXene nanofiber aerogel without the addition of Ag-Ag2S nanoparticles can only be degraded by the photodegradation properties of / MXene itself, and the degradation efficiency is not as high as that of adding sulfur and silver sulfide.

[0089] Test Example 1

[0090] The nanofiber aerogels obtained in Examples 1-4 and Comparative Example 2 were subjected to performance tests, and the test steps were as follows:

[0091] The PAN / MXene@Ag-Ag2S nanofiber aerogel prepared in the example was placed in a solution containing methylene blue or rhodamine 6G at a concentration of 1 mg / L-10 mg / L, and a photocatalytic degradation reaction occurred under visible light illumination (wherein Fig.10 The photodegradation rate is calculated by testing the absorbance of the solution after degradation.

[0092] Aerogels usually have a low density due to their porous structure. According to the following formula The volume density of the aerogel can be calculated; where m is the density of the aerogel, v is the mass of the aerogel, and is the volume of the aerogel (in the present invention, the aerogel is considered to be a regular cylindrical shape)

[0093] In addition, porosity is also one of the important indicators of aerogel. The porosity P (%) of PAN / MXene@Ag-Ag2S nanofiber aerogel can be calculated according to the formula Calculate. Where ρ is the density of the aerogel, ρ S is the density of the solid component. Since the main components of PAN / MXene@Ag-Ag2S nanofiber aerogel are PAN nanofibers and MXene, and other components are negligible, the density of the solid component is the density of PAN nanofibers (PAN = 1.3 mg / cm 3 The density of MXene aerogel is 8.7 mg / cm 3The density of PAN / / MXene@Ag-Ag2S nanofiber aerogel was calculated, and finally the porosity of PAN / / MXene@Ag-Ag2S nanofiber aerogel was calculated.

[0094] The test results are shown in Table 1:

[0095] Table 1

[0096]

[0097] From the data results in Table 1, we can see that:

[0098] (1) As the mass ratio of silver nitrate and thiourea loaded and reacted on the MXene surface changes from 2:1 to 3:1 and then to 4:1, the composite aerogels have abundant porosity and gradually increase, with the porosity being 94.2%, 95.7%, and 97.5%, respectively.

[0099] (2) As the mass ratio of silver nitrate and thiourea loaded and reacted on the MXene surface changes from 2:1 to 3:1 and then to 4:1, the density of the composite aerogel gradually increases, with the density being 23 mg / cm 3 、36mg / cm 3 and 42mg / cm 3 .

[0100] (3) As the mass ratio of silver nitrate and thiourea loaded and reacted on the MXene surface changes from 2:1 to 3:1 and then to 4:1, the composite aerogel has excellent photodegradation performance and gradually improves. The photodegradation rates of methylene blue are 95.56%, 96.87%, and 98.85%, respectively, and the photodegradation rates of rhodamine 6G are 92.73%, 93.61%, and 95.67%, respectively.

[0101] (4) As the mass ratio of silver nitrate and thiourea loaded and reacted on the MXene surface changed from 2:1 to 3:1 and then to 4:1, the time required for the photodegradation of the composite aerogel gradually shortened, and the time required for its complete photodegradation was 90 min, 60 min and 40 min.

[0102] (5) Compared with the PAN nanofibers and MXene@Ag-Ag2S with a mass ratio of 1:1 (Example 1), the porosity of Example 4 with a mass ratio of 2:1 increased to 98% and the aerogel length increased by 5 cm.

[0103] in, Fig.11 The spectrum of Rhodamine 6G dye before and after degradation at a concentration of 10 mg / L; Fig.12 The spectrum of Rhodamine 6G dye before and after degradation at a concentration of 1 mg / L; Fig.13The spectra of methylene blue dye before and after degradation at a concentration of 10 mg / L; Fig.14 The following is the spectrum of methylene blue dye before and after degradation at a concentration of 1 mg / L. Figures 11 to 14 It can be seen that PAN / MXene@Ag-Ag2S nanofiber aerogel can photodegrade methylene blue and rhodamine 6G organic dyes under light conditions, and the photocatalytic degradation rates are both above 90%, among which the highest degradation rates of methylene blue reach 98.85%, and the highest degradation rates of rhodamine 6G reach 95.67%.

[0104] The spectra of the polyacrylonitrile / MXene nanofiber aerogel prepared in Comparative Example 2 of the present invention before and after the degradation of methylene blue dye are as follows: Fig.16 As shown; the spectrum of the polyacrylonitrile / MXene nanofiber aerogel prepared in Comparative Example 2 of the present invention before and after the degradation of Rhodamine 6G dye is as shown Fig.17 shown by Fig.16 and Fig.17 It can be seen that PAN / MXene nanofiber aerogel without the addition of Ag-Ag2S nanoparticles can only rely on the photodegradation performance of / MXene itself for degradation, and the degradation efficiency is not as high as that of adding sulfur and silver sulfide. The degradation rate of methylene blue is 60.12%, and the degradation rate of rhodamine 6G is 37.53%.

[0105] Test Example 2

[0106] The nanofiber aerogel obtained in Example 1 was subjected to a cyclic photodegradation performance test, and the test steps were as follows:

[0107] The PAN / MXene@Ag-Ag2S nanofiber aerogel was placed in a methylene blue dye with a concentration of 1 mg / L, and a photocatalytic degradation reaction occurred under visible light illumination. The photodegradation rate was calculated by testing the absorbance of the solution after degradation. The aerogel after the first photodegradation was then taken out and washed, and the above operation was repeated to calculate the photodegradation rate, which was repeated three times in total.

[0108] The photodegradation rate of polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel prepared in Example 1 of the present invention after cyclic degradation is shown in the figure Fig.15 shown by Fig.15 It can be seen that after PAN / MXene@Ag-Ag2S nanofiber aerogel has been photocatalytically degraded three times with a concentration of 1 mg / L of methylene blue dye, the photocatalytic degradation rate remains above 90%, showing good reusability.

[0109] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel, characterized in that: The polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel consists of polyacrylonitrile nanofibers, MXene and Ag-Ag2S nanoparticles loaded on MXene; the polyacrylonitrile nanofibers are bonded to MXene through hydrogen bonds; the polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel is a three-dimensional porous structure with a porosity of 94.2% to 97.5%.

2. The polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel according to claim 1, characterized in that: The diameter of the Ag-Ag2S nanoparticles is 10nm to 500nm.

3. A method for preparing polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel, characterized in that: The following steps are involved: (1) MXene powder is dissolved in water, and the precipitate obtained after centrifugation is dispersed in water by ultrasound, repeated oscillation and centrifugation to obtain a flaky MXene dispersion; (2) adding silver nitrate, thiourea and alkali to the flaked MXene dispersion obtained in step (1), mixing and reacting under light conditions to obtain a MXene@Ag-Ag2S dispersion; (3) Mixing the alkaline hydrolyzed polyacrylonitrile nanofibers with the MXene@Ag-Ag2S dispersion obtained in step (2) to obtain the polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel.

4. The preparation method according to claim 3, characterized in that: In step (2), the illumination time is 3 h to 5 h.

5. The preparation method according to claim 3, characterized in that: In step (2), the mass ratio of the silver nitrate, thiourea and alkali is 2-4:1:

1.

6. The preparation method according to claim 3, characterized in that: In step (3), the mass ratio of the alkaline hydrolyzed polyacrylonitrile nanofibers to the MXene@Ag-Ag2S dispersion is 1 to 2:

1.

7. The preparation method according to claim 3, characterized in that: In step (3), the alkaline hydrolyzed polyacrylonitrile nanofibers are prepared by the following method: S1, heating and dissolving polyacrylonitrile in an organic solvent to obtain a polyacrylonitrile spinning solution, and preparing a polyacrylonitrile nanofiber membrane by electrospinning; cutting the polyacrylonitrile nanofiber membrane into pieces, and homogenizing it in water to obtain a polyacrylonitrile nanofiber dispersion; S2, adding the polyacrylonitrile nanofiber dispersion obtained in step S1 into an alkaline solution for heating and alkaline hydrolysis for 20 minutes to 30 minutes to obtain the alkaline-hydrolyzed polyacrylonitrile nanofibers.

8. Use of the polyacrylonitrile / MXene@Ag-Ag2S nanofiber aerogel according to claim 1 or 2 in degrading dyes.

9. The use according to claim 8, characterized in that: The concentration of the dye is 1 mg / L-10 mg / L.