A method for effectively inhibiting lithium volatilization in lithium orthosilicate ceramic balls

Through the gel injection molding process and high-temperature sintering technology of lithium alginate and polyvinyl alcohol, the problem of lithium metasilicate formation caused by lithium volatilization was solved, and lithium orthosilicate ceramic pellets with high crushing load and density that met the specifications were prepared. , meeting the performance requirements of tritium-proliferated ceramic balls.

CN116535201BActive Publication Date: 2024-10-18KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310421959.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-18
Estimated Expiration
2043-04-19

AI Technical Summary

Technical Problem

In the process of preparing lithium orthosilicate ceramic pellets, the volatility of lithium leads to the formation of lithium metasilicate, and the phase purity cannot meet the index requirements. The existing method has the problem of inconsistent crushing load and density.

Method used

Ceramic pellets are prepared using materials such as lithium alginate and polyvinyl alcohol through a gel injection molding process. Through liquid nitrogen freezing and sintering processes, the sintering conditions are controlled to inhibit lithium volatilization and ensure the density and performance of the pellets.

Benefits of technology

A lithium orthosilicate ceramic pellet with a crushing load of 35N and a relative density of 85% has been achieved, which meets the performance indicators of tritium-proliferated ceramic pellets and ensures the purity and density of the pellets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004187180630000051
    Figure BDA0004187180630000051
  • Figure BDA0004187180630000081
    Figure BDA0004187180630000081
  • Figure HDA0004187180640000011
    Figure HDA0004187180640000011
Patent Text Reader

Abstract

The present invention relates to a method for effectively inhibiting the volatilization of lithium in lithium orthosilicate ceramic spheres, and belongs to the technical field of ceramic materials. The present invention mixes lithium carbonate and nano-silicon dioxide, and then places the mixture at a temperature of 800-1000°C for solid phase reaction to obtain a lithium orthosilicate powder precursor; the lithium orthosilicate powder precursor, PVA aqueous solution and lithium alginate aqueous solution are evenly mixed to obtain a mixed slurry, and the mixed slurry is dripped into liquid nitrogen drop by drop to quench to obtain frozen microspheres, and the frozen microspheres are placed in an acetone solution, and vacuum dried until the acetone solution is completely volatilized to obtain ceramic spheres; the ceramic spheres are sintered at 400-600°C for 0.5-1.5h, and then sintered at 900-1100°C for 2-6h to obtain lithium orthosilicate tritium breeding ceramic spheres. The present invention utilizes lithium alginate to effectively inhibit the volatilization of lithium during the sintering process, and prepares ceramic balls with high phase purity. The crushing load of the ceramic balls far exceeds the performance index requirements of tritium breeding ceramic balls, and the density thereof also reaches the relevant index, satisfying the relevant performance indexes of tritium breeding ceramic balls.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for effectively inhibiting the volatilization of lithium in lithium orthosilicate ceramic beads, belonging to the technical field of ceramic materials. Background Art

[0002] Nuclear fusion reactions can produce much more energy than the energy provided by starting the reaction process, resulting in an overall increase in power. A nuclear fusion test reactor that can self-sustain combustion (i.e. "ignite") is used to verify the feasibility of a fusion reactor. The purpose of testing the Tritium Production Experimental Blanket Module (TBM) is to verify the production of tritium and energy in commercial fusion reactors. Lithium orthosilicate (Li4SiO4) is currently considered to be one of the most important candidate materials for the breeder blanket of thermonuclear fusion reactors due to its high lithium density, high thermal conductivity, good stability, and tritium release rate.

[0003] The basic requirements of TBM (test blanket module) for solid tritium breeder are that the diameter of the ball is between 1 and 2 mm, the crushing load is greater than 10N, and the relative density is greater than 80%. At present, the preparation methods of lithium orthosilicate balls mainly include sol-gel method, melt spray method, graphite ball bed method, etc. However, the lithium orthosilicate ceramic balls prepared by the above methods all have various problems. The crushing load of lithium orthosilicate balls prepared by sol-gel method can reach 40N, but the density cannot meet the index requirements, only 74%; the relative density of lithium orthosilicate balls prepared by melt spray method can reach 95%, but the crushing load is only 7 to 20N, and the crushing load of lithium orthosilicate balls prepared by graphite ball bed method can reach 60N, but the sphericity cannot meet the requirements. However, the common problem of all methods is that due to the volatility of lithium during the preparation process, lithium metasilicate will be generated, and the phase purity cannot meet the index requirements. Summary of the invention

[0004] In view of the problem that the volatility of lithium in the preparation process of solid tritium breeder lithium orthosilicate beads will lead to the generation of lithium metasilicate, and the phase purity cannot meet the index requirements, the present invention proposes a method for effectively inhibiting the volatilization of lithium in lithium orthosilicate ceramic beads, that is, using lithium alginate organic matter, using gel injection molding process, ceramic powder and polyvinyl alcohol, lithium alginate solution are mixed in a specific ratio, and the prepared slurry is dripped into liquid nitrogen by dripping. During the falling process, the droplets shrink into a spherical shape under the action of gravity and surface tension; then the frozen beads are immersed in acetone and dried to obtain a ceramic bead blank with a certain strength, and finally the lithium orthosilicate ceramic beads are obtained by sintering process. The process of the present invention is simple and safe, the crushing load of the prepared beads can reach 35N, the relative density is 85%, and it can be produced continuously with high production efficiency.

[0005] A method for effectively inhibiting the volatilization of lithium in lithium orthosilicate ceramic balls, the specific steps are as follows:

[0006] (1) mixing lithium carbonate and nano-silicon dioxide, and then subjecting the mixture to a solid phase reaction at a temperature of 800 to 1000° C. to obtain a lithium orthosilicate powder precursor;

[0007] (2) mixing a lithium orthosilicate powder precursor, a PVA aqueous solution and a lithium alginate aqueous solution to obtain a mixed slurry;

[0008] (3) dropping the mixed slurry dropwise into liquid nitrogen to quench it to obtain frozen microspheres;

[0009] (4) placing the frozen microspheres in an acetone solution and vacuum drying until the acetone solution is completely evaporated to obtain ceramic microspheres;

[0010] (5) The ceramic spheres are heated uniformly to 400-600°C and sintered at this temperature for 0.5-1.5 hours, and then heated uniformly to 900-1100°C and sintered at this temperature for 2-6 hours to obtain lithium orthosilicate tritium breeding ceramic spheres. The two-stage sintering process can not only completely volatilize the organic matter in the microspheres, but also ensure that the particles in the lithium orthosilicate spheres adhere to each other, shrink in volume and quickly densify to form a solid sintered body, thus ensuring the density of the spheres and the loading and adsorption properties of the lithium orthosilicate material.

[0011] In the step (1), the molar ratio of lithium carbonate to nano-silicon dioxide is 2:1.

[0012] In the step (2), the mass concentration of the PVA aqueous solution is 3%, and the mass concentration of the lithium alginate aqueous solution is 1-3%. In terms of mass percentage, the lithium orthosilicate powder precursor accounts for 50-70% of the mixed slurry, the lithium alginate aqueous solution accounts for 10%, and the rest is the PVA aqueous solution.

[0013] The mixed slurry in step (3) is added dropwise into liquid nitrogen through a needle with an inner diameter of 0.5 to 1.5 mm, wherein the inner diameter of the needle is used to control the particle size of the frozen microspheres.

[0014] The particle size of the frozen microspheres in step (3) is 1.5 mm to 2 mm.

[0015] The upper liquid surface of the acetone solution in step (4) is 0.5 to 1 cm higher than the top surface of the frozen microspheres, so that the ceramic microspheres do not agglomerate and can be better shaped.

[0016] The vacuum drying temperature in step (4) is 50-70°C.

[0017] The uniform heating rate in step (5) is 3-5°C / min.

[0018] The principle of the present invention for effectively inhibiting the volatilization of lithium in the lithium orthosilicate ceramic beads is that by adding lithium alginate, it can react with impurities such as lithium metasilicate generated and contained in the lithium orthosilicate reaction process and in the precursor powder, thereby generating lithium orthosilicate, removing impurities, and replenishing lithium orthosilicate, thereby achieving the effect of inhibiting the volatilization of lithium in the lithium orthosilicate ceramic beads during the sintering process.

[0019] The beneficial effects of the present invention are:

[0020] (1) The present invention uses polyethylene glycol PVA and lithium alginate as binders for preparing ceramic balls, which are non-toxic, rational, and environmentally friendly;

[0021] (2) The present invention adopts the gel dripping method to prepare lithium orthosilicate ceramic spheres, the crushing strength of which can reach 35N and the relative density can reach 85%, meeting the performance indicators of tritium breeding ceramic spheres;

[0022] (3) The present invention uses lithium alginate to inhibit the volatilization of lithium during the sintering process of ball forming, and substances such as C, O, and H in lithium alginate will completely volatilize during the sintering process, and will not produce impurities such as lithium metasilicate, and the phase purity can meet the requirements;

[0023] (4) The high-temperature sintering of the present invention completely volatilizes the organic matter in the microspheres, ensuring that the particles in the lithium orthosilicate spheres adhere to each other, shrink in volume and densify rapidly to form a strong sintered body, and ensuring the density of the spheres and the loading and adsorption properties of the lithium orthosilicate material. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Li sintered by solid phase method in Example 1 4 SiO 4 XRD pattern of precursor powder;

[0025] Figure 2 is the Li after sintering in Example 1 4 SiO 4 Pictures of small balls;

[0026] Figure 3 is the Li after sintering in Example 1 4 SiO 4 XRD pattern of pellets;

[0027] Figure 4 Li before and after sintering in Example 1 4 SiO 4 SEM images of the ball surface, left is before sintering, right is after sintering;

[0028] Figure 5 is the Li after sintering in Example 2 4 SiO 4 Pictures of small balls;

[0029] Figure 6 is the Li after sintering in Example 2 4 SiO 4 XRD pattern of pellets;

[0030] Figure 7 Li before and after sintering in Example 2 4 SiO 4 SEM images of the ball surface, left is before sintering, right is after sintering;

[0031] Figure 8 is the Li after sintering in Example 3 4 SiO 4 Pictures of small balls;

[0032] Fig. 9 is the Li after sintering in Example 3 4 SiO 4 XRD pattern of pellets;

[0033] Fig.10 Li before and after sintering in Example 3 4 SiO 4 SEM images of the ball surface, left is before sintering, right is after sintering;

[0034] Fig.11 The crushing load and density diagrams of Examples 1 to 3;

[0035] Fig.12 is the Li after sintering in Example 4 4 SiO 4 XRD pattern of pellets;

[0036] Fig.13 is the Li after sintering in Example 4 4 SiO 4 SEM image of the ball surface;

[0037] Fig.14 is the Li after sintering in Example 5 4 SiO 4 XRD pattern of pellets;

[0038] Fig.15 is the Li after sintering in Example 5 4 SiO 4 SEM image of the ball surface;

[0039] Fig.16 is the Li after sintering in Example 6 4 SiO 4 XRD pattern of pellets;

[0040] Fig.17is the Li after sintering in Example 6 4 SiO 4 SEM image of the ball surface;

[0041] Fig.18 The crushing load and density diagrams of Examples 4 to 6 are shown. DETAILED DESCRIPTION

[0042] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.

[0043] Example 1: A method for effectively inhibiting the volatilization of lithium in lithium orthosilicate ceramic spheres, the specific steps are as follows:

[0044] (1) lithium carbonate and nano-silicon dioxide were mixed, and then placed at a temperature of 900°C for solid phase reaction for 120 minutes, cooled to room temperature, and ground through a 200-mesh sieve to obtain a lithium orthosilicate powder precursor; wherein the molar ratio of lithium carbonate to nano-silicon dioxide was 2:1; the Li2O3 sintered by the solid phase method in this embodiment 4 SiO 4 The XRD pattern of the precursor powder is shown in Figure 1 ,from Figure 1 It can be seen that the solid phase sintered Li 4 SiO 4 The precursor powder is relatively pure and contains a small amount of Li 2 SiO 3 , through JADE6.0 analysis, we can get 4 SiO 4 The content of Li can reach 99.5wt%, 2 SiO 3 The content is 0.5wt%, so the precursor powder prepared by the solid phase method can meet the needs of preparing tritium breeding ceramic balls.

[0045] (2) mixing a lithium orthosilicate powder precursor, a PVA aqueous solution and a lithium alginate aqueous solution to obtain a mixed slurry; wherein the mass concentration of the polyethylene glycol PVA aqueous solution is 3%, the mass concentration of the lithium alginate aqueous solution is 1%, and the mass ratio of the lithium orthosilicate powder precursor, the PVA aqueous solution and the lithium alginate aqueous solution is 6:3:1;

[0046] (3) dripping the mixed slurry into liquid nitrogen drop by drop through a needle with an inner diameter of 1.5 mm to quench the mixture to obtain frozen microspheres; wherein the particle size of the frozen microspheres is 2 mm to 2.3 mm;

[0047] (4) placing the frozen microspheres in an acetone solution so that the upper liquid level of the acetone solution is 0.5 cm higher than the top surface of the frozen microspheres, and placing them in a vacuum dryer at a temperature of 70° C. until the acetone solution is completely evaporated to obtain ceramic microspheres;

[0048] (5) the ceramic ball is heated to 500°C at a heating rate of 3°C / min and sintered at this temperature for 1 hour, then heated to 900°C at a heating rate of 3°C / min and sintered at this temperature for 5 hours, and then cooled in the furnace to obtain lithium orthosilicate tritium breeding ceramic ball;

[0049] The lithium orthosilicate tritium breeding ceramic spheres after sintering in this embodiment are shown in FIG. Figure 2 ,from Figure 2 It can be seen that the balls photographed by the digital camera have good sphericity, and some balls have micro-pits;

[0050] The XRD pattern of the lithium orthosilicate tritium-breeding ceramic spheres after sintering in this example is shown in FIG. Figure 3 ,from Figure 3 It can be seen that the phase after sintering is relatively pure Li 4 SiO 4 This indicates that the addition of lithium alginate can effectively remove the Li 2 SiO 3 Remove and inhibit the volatilization of lithium in lithium orthosilicate ceramic beads. By JDAE6.0 analysis, Li 4 SiO 4 The content reaches 99.6wt%;

[0051] The SEM image of the lithium orthosilicate tritium breeding ceramic sphere after sintering in this embodiment is shown in Figure 4 , the left is before sintering, the right is after sintering, Figure 4 It can be seen that after sintering, the cracks on the surface of the balls increase, the bonding effect between the particles is poor, and there are a large number of holes. This is because when the PVA solution and the lithium alginate solution are combined with the balls, the PVA solution accounts for the majority, which leads to the volatilization of organic matter during the sintering process, making the bonding between the particles of the balls more difficult, resulting in an increase in holes and cracks.

[0052] Example 2: A method for effectively inhibiting the volatilization of lithium in lithium orthosilicate ceramic balls, the specific steps are as follows:

[0053] (1) mixing lithium carbonate and nano-silicon dioxide, and then placing the mixture at 800° C. for solid phase reaction for 120 min, cooling to room temperature, and grinding the mixture through a 200-mesh sieve to obtain a lithium orthosilicate powder precursor; wherein the molar ratio of lithium carbonate to nano-silicon dioxide is 2:1;

[0054] (2) mixing a lithium orthosilicate powder precursor, a PVA aqueous solution and a lithium alginate aqueous solution to obtain a mixed slurry; wherein the mass concentration of the polyethylene glycol PVA aqueous solution is 3%, the mass concentration of the lithium alginate aqueous solution is 2%, and the mass ratio of the lithium orthosilicate powder precursor, the PVA aqueous solution and the lithium alginate aqueous solution is 6:3:1;

[0055] (3) dripping the mixed slurry into liquid nitrogen drop by drop through a needle with an inner diameter of 1.5 mm to quench the mixture to obtain frozen microspheres; wherein the particle size of the frozen microspheres is 2 mm to 2.3 mm;

[0056] (4) placing the frozen microspheres in an acetone solution so that the upper liquid level of the acetone solution is 0.8 cm higher than the top surface of the frozen microspheres, and placing them in a vacuum dryer at a temperature of 70° C. until the acetone solution is completely evaporated to obtain ceramic microspheres;

[0057] (5) the ceramic ball is heated to 500°C at a heating rate of 3°C / min and sintered at this temperature for 1 hour, then heated to 1000°C at a heating rate of 3°C / min and sintered at this temperature for 5 hours, and then cooled in the furnace to obtain lithium orthosilicate tritium breeding ceramic ball;

[0058] The lithium orthosilicate tritium breeding ceramic spheres after sintering in this embodiment are shown in FIG. Figure 5 ,from Figure 5 It can be seen that the balls have good sphericity and some of them have micro-pits on their surfaces;

[0059] The XRD pattern of the lithium orthosilicate tritium-breeding ceramic spheres after sintering in this example is shown in FIG. Figure 6 ,from Figure 6 It can be seen that the phase after sintering is relatively pure Li 4 SiO 4 , and no miscellaneous items appear. Through JDAE6.0 analysis, Li 4 SiO 4 The content reaches 99.8wt%;

[0060] The SEM image of the lithium orthosilicate tritium breeding ceramic sphere after sintering in this embodiment is shown in Figure 7 , the left is before sintering, the right is after sintering, Figure 7 It can be seen that the cracks on the surface of the balls increased after sintering, and the bonding effect between the particles was better. This is because with the increase of lithium alginate content, the balls bonded with Li in the precursor powder during the sintering process. 2 SiO 3 Reaction, generating Li 4 SiO 4 , it is replenished into the organic cracks occupied by PVA, but it cannot completely fill the cracks, so cracks and small holes are generated.

[0061] Example 3: A method for effectively inhibiting the volatilization of lithium in lithium orthosilicate ceramic balls, the specific steps are as follows:

[0062] (1) mixing lithium carbonate and nano-silicon dioxide, and then placing the mixture at a temperature of 1000° C. for solid phase reaction for 120 minutes, cooling to room temperature, and grinding the mixture through a 200-mesh sieve to obtain a lithium orthosilicate powder precursor; wherein the molar ratio of lithium carbonate to nano-silicon dioxide is 2:1;

[0063] (2) mixing a lithium orthosilicate powder precursor, a PVA aqueous solution and a lithium alginate aqueous solution to obtain a mixed slurry; wherein the mass concentration of the polyethylene glycol PVA aqueous solution is 3%, the mass concentration of the lithium alginate aqueous solution is 3%, and the mass ratio of the lithium orthosilicate powder precursor, the PVA aqueous solution and the lithium alginate aqueous solution is 6:3:1;

[0064] (3) dripping the mixed slurry into liquid nitrogen drop by drop through a needle with an inner diameter of 1.5 mm to quench the mixture to obtain frozen microspheres; wherein the particle size of the frozen microspheres is 2 mm to 2.3 mm;

[0065] (4) placing the frozen microspheres in an acetone solution so that the upper liquid level of the acetone solution is 1.0 cm higher than the top surface of the frozen microspheres, and placing them in a vacuum dryer at a temperature of 70° C. until the acetone solution is completely evaporated to obtain ceramic microspheres;

[0066] (5) the ceramic ball is heated to 500°C at a heating rate of 3°C / min and sintered at this temperature for 1 hour, then heated to 1100°C at a heating rate of 3°C / min and sintered at this temperature for 5 hours, and then cooled in the furnace to obtain lithium orthosilicate tritium breeding ceramic ball;

[0067] The lithium orthosilicate tritium breeding ceramic spheres after sintering in this embodiment are shown in FIG. Figure 8 ,from Figure 8 It can be seen that the balls have good sphericity and some of them have micro-pits on their surfaces;

[0068] The XRD pattern of the lithium orthosilicate tritium-breeding ceramic spheres after sintering in this example is shown in FIG. Fig. 9 ,from Fig. 9 It can be seen that the phase after sintering is relatively pure Li 4 SiO 4 , and no miscellaneous items appear. Through JDAE6.0 analysis, Li 4 SiO 4 The content reaches 99.8wt%;

[0069] The SEM image of the lithium orthosilicate tritium breeding ceramic sphere after sintering in this embodiment is shown in Fig.10 , the left is before sintering, the right is after sintering, Fig.10 It can be seen that after sintering, the cracks on the surface of the balls are reduced, the bonding effect between the particles is good, and there are micropores. This is because as the lithium alginate content further increases, the balls react with the Li in the precursor powder during the sintering process. 2 SiO 3 Reaction, generating Li 4 SiO 4 , replenished into the cracks of organic matter occupied by PVA, making the particles more closely bonded and the grains better bonded;

[0070] The lithium content in the lithium orthosilicate tritium breeding ceramic spheres after sintering in Examples 1 to 3 is shown in Table 1.

[0071] Table 1 Lithium content in lithium orthosilicate tritium breeding ceramic spheres after sintering of Examples 1 to 3

[0072]

[0073] Compared with the lithium orthosilicate powder precursor, the lithium content in the lithium orthosilicate tritium breeder ceramic beads increased after sintering, and increased with the increase of lithium alginate addition;

[0074] The crushing load and density diagrams of Examples 1 to 3 are shown in Fig.11 ,from Fig.11 It can be seen that with the increase of lithium alginate content, the crushing strength and density of lithium orthosilicate tritium breeding ceramic spheres will increase. Among them, the crushing strength and density of 3wt% lithium alginate are the largest, with a crushing strength of 35N and a density of 1.97g / cm 3 , which shows that adding lithium alginate can effectively improve the crushing strength and density of the balls.

[0075] Example 4: A method for effectively inhibiting the volatilization of lithium in lithium orthosilicate ceramic balls, the specific steps are as follows:

[0076] (1) mixing lithium carbonate and nano-silicon dioxide, and then placing the mixture at 800° C. for solid phase reaction for 120 min, cooling to room temperature, and grinding the mixture through a 200-mesh sieve to obtain a lithium orthosilicate powder precursor; wherein the molar ratio of lithium carbonate to nano-silicon dioxide is 2:1;

[0077] (2) mixing a lithium orthosilicate powder precursor, a PVA aqueous solution and a lithium alginate aqueous solution to obtain a mixed slurry; wherein the mass concentration of the polyethylene glycol PVA aqueous solution is 3%, the mass concentration of the lithium alginate aqueous solution is 3%, and the mass ratio of the lithium orthosilicate powder precursor, the PVA aqueous solution and the lithium alginate aqueous solution is 6:3:1;

[0078] (3) dripping the mixed slurry into liquid nitrogen dropwise through a needle with an inner diameter of 1.2 mm to quench the mixture to obtain frozen microspheres; wherein the particle size of the frozen microspheres is 1.8 to 2 mm;

[0079] (4) placing the frozen microspheres in an acetone solution so that the upper liquid level of the acetone solution is 0.8 cm higher than the top surface of the frozen microspheres, and placing them in a vacuum dryer at a temperature of 50° C. until the acetone solution is completely evaporated to obtain ceramic microspheres;

[0080] (5) The ceramic ball is heated to 400°C at a heating rate of 4°C / min and sintered at this temperature for 0.5h, then heated to 1000°C at a heating rate of 4°C / min and sintered at this temperature for 6h, and then cooled in the furnace to obtain lithium orthosilicate tritium breeding ceramic ball;

[0081] The XRD pattern of the lithium orthosilicate tritium-breeding ceramic spheres after sintering in this example is shown in FIG. Fig.12 ,from Fig.12 It can be seen that the phase after sintering is relatively pure Li 4 SiO 4 , and no miscellaneous items appear. Through JDAE6.0 analysis, Li 4 SiO 4 The content reaches 99.8wt%;

[0082] The SEM image of the lithium orthosilicate tritium breeding ceramic sphere after sintering in this embodiment is shown in Fig.13 , the left is before sintering, the right is after sintering, Fig.13 It can be seen that after sintering, the cracks on the surface of the balls are reduced, the bonding effect between the particles is good, and micropores exist. This is because as the temperature increases, the particle regrowth effect is good, and the bonding between the particles is tighter, resulting in a reduction in cracks and the best effect. Compared with the lithium orthosilicate powder precursor, the lithium content in the lithium orthosilicate tritium breeding ceramic balls after sintering increases to 28.51wt%.

[0083] Example 5: A method for effectively inhibiting the volatilization of lithium in lithium orthosilicate ceramic spheres, the specific steps are as follows:

[0084] (1) mixing lithium carbonate and nano-silicon dioxide, and then placing the mixture at 900° C. for solid phase reaction for 120 min, cooling to room temperature, and grinding the mixture through a 200-mesh sieve to obtain a lithium orthosilicate powder precursor; wherein the molar ratio of lithium carbonate to nano-silicon dioxide is 2:1;

[0085] (2) mixing a lithium orthosilicate powder precursor, a PVA aqueous solution and a lithium alginate aqueous solution to obtain a mixed slurry; wherein the mass concentration of the polyethylene glycol PVA aqueous solution is 3%, the mass concentration of the lithium alginate aqueous solution is 3%, and the mass ratio of the lithium orthosilicate powder precursor, the PVA aqueous solution and the lithium alginate aqueous solution is 7:2:1;

[0086] (3) dripping the mixed slurry into liquid nitrogen drop by drop through a needle with an inner diameter of 1.0 mm to quench the mixture to obtain frozen microspheres; wherein the particle size of the frozen microspheres is 1.5 mm to 1.8 mm;

[0087] (4) placing the frozen microspheres in an acetone solution so that the upper liquid level of the acetone solution is 1.0 cm higher than the top surface of the frozen microspheres, and placing them in a vacuum dryer at a temperature of 60° C. until the acetone solution is completely evaporated to obtain ceramic microspheres;

[0088] (5) The ceramic ball is heated to 600°C at a heating rate of 3°C / min and sintered at this temperature for 1.5 hours, then heated to 1100°C at a heating rate of 5°C / min and sintered at this temperature for 6 hours, and then cooled in the furnace to obtain lithium orthosilicate tritium breeding ceramic ball;

[0089] The XRD pattern of the lithium orthosilicate tritium-breeding ceramic spheres after sintering in this example is shown in FIG. Fig.14 ,from Fig.14 It can be seen that the phase after sintering is relatively pure Li 4 SiO 4 , and no miscellaneous items appear. Through JDAE6.0 analysis, Li 4 SiO 4 The content reaches 99.8wt%;

[0090] The SEM image of the lithium orthosilicate tritium breeding ceramic sphere after sintering in this embodiment is shown in Fig.15 , the left is before sintering, the right is after sintering, Fig.15 It can be seen that after sintering, the cracks on the surface of the balls are reduced, the bonding effect between the particles is good, and micropores exist. This is because as the temperature increases, the particle regrowth effect is good, and the bonding between the particles is tighter, resulting in fewer cracks and making the balls denser. Compared with the lithium orthosilicate powder precursor, the lithium content in the lithium orthosilicate tritium breeding ceramic balls after sintering increases to 26.19wt%.

[0091] Example 6: A method for effectively inhibiting the volatilization of lithium in lithium orthosilicate ceramic spheres, the specific steps are as follows:

[0092] (1) mixing lithium carbonate and nano-silicon dioxide, and then placing the mixture at a temperature of 1000° C. for solid phase reaction for 120 minutes, cooling to room temperature, and grinding the mixture through a 200-mesh sieve to obtain a lithium orthosilicate powder precursor; wherein the molar ratio of lithium carbonate to nano-silicon dioxide is 2:1;

[0093] (2) mixing a lithium orthosilicate powder precursor, a PVA aqueous solution and a lithium alginate aqueous solution to obtain a mixed slurry; wherein the mass concentration of the polyethylene glycol PVA aqueous solution is 3%, the mass concentration of the lithium alginate aqueous solution is 2%, and the mass ratio of the lithium orthosilicate powder precursor, the PVA aqueous solution and the lithium alginate aqueous solution is 5:4:1;

[0094] (3) dripping the mixed slurry into liquid nitrogen dropwise through a needle with an inner diameter of 0.8 mm to quench the mixture to obtain frozen microspheres; wherein the particle size of the frozen microspheres is 1.4 to 1.6 mm;

[0095] (4) placing the frozen microspheres in an acetone solution so that the upper liquid level of the acetone solution is 1.0 cm higher than the top surface of the frozen microspheres, and placing them in a vacuum dryer at a temperature of 50° C. until the acetone solution is completely evaporated to obtain ceramic microspheres;

[0096] (5) The ceramic ball is heated to 500° C. at a heating rate of 5° C. / min and sintered at this temperature for 1 hour, then heated to 900° C. at a heating rate of 4° C. / min and sintered at this temperature for 6 hours, and then cooled in the furnace to obtain lithium orthosilicate tritium breeding ceramic ball;

[0097] The XRD pattern of the lithium orthosilicate tritium-breeding ceramic spheres after sintering in this example is shown in FIG. Fig.16 ,from Fig.16 It can be seen that the phase after sintering is relatively pure Li 4 SiO 4 , and no miscellaneous items appear. Through JDAE6.0 analysis, Li 4 SiO 4 The content reaches 99.7wt%;

[0098] The SEM image of the lithium orthosilicate tritium breeding ceramic sphere after sintering in this embodiment is shown in Fig.17 , the left is before sintering, the right is after sintering, Fig.17 It can be seen that after sintering, the cracks on the surface of the ball are reduced, the bonding effect between the particles is better, and there are micropores. This is because as the sintering temperature increases, the organic matter will volatilize, and the particles will combine with each other, but due to the low temperature, the particles cannot grow again and combine better with other particles. In addition, due to the excessive content of organic matter, the pores between the particles will gradually increase, so cracks will appear. Compared with the lithium orthosilicate powder precursor, the lithium content in the lithium orthosilicate tritium breeding ceramic ball after sintering increases to 24.85wt%;

[0099] The lithium content in the lithium orthosilicate tritium breeding ceramic spheres after sintering in Examples 4 to 6 is shown in Table 2.

[0100] Table 2 Lithium content in lithium orthosilicate tritium breeding ceramic spheres after sintering of Examples 4 to 6

[0101]

[0102] Compared with the lithium orthosilicate powder precursor, the lithium content in the lithium orthosilicate tritium breeder ceramic pellets increased after sintering, and the Li content increased the most at 1000℃;

[0103] The crushing load and density diagrams of Examples 4 to 6 are shown in Fig.18 ,from Fig.18 It can be seen that when the content of lithium alginate and PVA is constant, it can be seen that with the increase of sintering temperature, the crushing strength and density of lithium orthosilicate tritium breeder ceramic spheres will also increase accordingly, that is, the sintering temperature and lithium orthosilicate tritium breeder ceramic spheres have a linear growth relationship, that is, the higher the sintering temperature, the greater the crushing load and density of the spheres, and the better the performance.

[0104] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.

Claims

1. A method for effectively inhibiting the volatilization of lithium in lithium orthosilicate ceramic beads, characterized in that: The specific steps are as follows: (1) mixing lithium carbonate and nano-silicon dioxide, and then subjecting the mixture to a solid phase reaction at a temperature of 800 to 1000° C. to obtain a lithium orthosilicate powder precursor; (2) mixing the lithium orthosilicate powder precursor, the PVA aqueous solution and the lithium alginate aqueous solution to obtain a mixed slurry; (3) dripping the mixed slurry drop by drop into liquid nitrogen to quench and obtain frozen microspheres; the mass concentration of the PVA aqueous solution is 3%, the mass concentration of the lithium alginate aqueous solution is 2-3%, and in terms of mass percentage, the lithium orthosilicate powder precursor accounts for 60-80% of the mixed slurry, the lithium alginate aqueous solution accounts for 10%, and the rest is the PVA aqueous solution; (4) placing the frozen microspheres in an acetone solution and vacuum drying until the acetone solution is completely evaporated to obtain ceramic microspheres; (5) The temperature of the ceramic ball is uniformly raised to 400-600° C. and sintered at the temperature for 0.5-1.5 h, and then the temperature is uniformly raised to 1000-1100° C. and sintered at the constant temperature for 2-6 h to obtain lithium orthosilicate tritium breeding ceramic ball.

2. The method for effectively inhibiting the volatilization of lithium in lithium orthosilicate ceramic beads according to claim 1, characterized in that: The molar ratio of lithium carbonate to nano-silicon dioxide in step (1) is 2:

1.

3. The method for effectively inhibiting the volatilization of lithium in lithium orthosilicate ceramic beads according to claim 1, characterized in that: The particle size of the frozen microspheres in step (3) is 1.5 mm to 2 mm.

4. The method for effectively inhibiting the volatilization of lithium in lithium orthosilicate ceramic beads according to claim 1, characterized in that: The upper liquid surface of the acetone solution in step (4) is 0.5 to 1 cm higher than the top surface of the frozen microspheres.

5. The method for effectively inhibiting the volatilization of lithium in lithium orthosilicate ceramic beads according to claim 1, characterized in that: The vacuum drying temperature in step (4) is 50-70°C.

6. The method for effectively inhibiting the volatilization of lithium in lithium orthosilicate ceramic beads according to claim 1, characterized in that: The uniform heating rate in step (5) is 3-5°C / min.