KrF photoresist and preparation method and patterning method thereof

By forming a chain structure through hyperbranched photoacid polymer resin, encapsulating photoacid groups and grafting at the tail end of the chain, the problem of degradation of photoresist resolution and LER performance is solved, and higher sensitivity and contrast are achieved. Reduces defects and side reactions in the resin structure.

CN116540493BActive Publication Date: 2024-11-12XIAMEN HENGKUN NEW MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310568802.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-12
Estimated Expiration
2043-05-19

AI Technical Summary

Technical Problem

During the exposure development process, existing photoresist has reduced resolution due to the volatilization and diffusion of PAG and photoacid, molecular chain entanglement has decreased resolution and LER performance, and resin structural defects have resulted in uneven resolution.

Method used

Hyperbranched photoacid polymerization resin is adopted to form a chain structure by hyperbranching polymerization of polyols, para-hydroxystyrene monomers, alkenyl tert-butyl ester, and photoacid monomers, forming a chain structure, encapsulating photoacid groups, and reducing protonic acid Diffusion and 4-(1-phenyl-1-hydroxyethyl)styrene is grafted at the tail end of the chain to reduce molecular chain entanglement and improve the uniformity of the resin structure.

Benefits of technology

The resolution and LER performance of the photoresist are improved, the Tg value is reduced, the sensitivity and contrast are enhanced, the T-top phenomenon is reduced, the side reactions are avoided, and the overall performance of the photoresist is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116540493B_ABST
    Figure CN116540493B_ABST
Patent Text Reader

Abstract

The present invention provides a KrF photoresist, characterized in that: by weight percentage, it includes 48.5-60.5% of hyperbranched photoacid polymerized resin, 0.5-1% of quencher, 0.03-0.5% of leveling agent, and 50%-72% of solvent; the hyperbranched photoacid polymerized resin is prepared by hyperbranched polymerization of polyol, p-hydroxystyrene monomer, alkenyl tert-butyl ester, photoacid monomer, and 4-(1-phenyl-1-hydroxyethyl) styrene; the 4-(1-phenyl-1-hydroxyethyl) styrene is hyperbranched grafted polymerized in the end group region after the p-hydroxystyrene monomer, alkenyl tert-butyl ester, and photoacid monomer are polymerized. At the same time, the present invention also provides a preparation method of KrF photoresist and a patterning method thereof. The chain structure of the present invention can reduce the diffusion of proton acid generated by the group of the photoacid to the non-exposed area and reduce the entanglement of molecular chains, improve resolution, LER performance, and reduce Tg value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photoresists, and in particular to a KrF photoresist and a preparation method and a patterning method thereof. Background Art

[0002] There is a balance between the resolution, line edge roughness (LER) and sensitivity of photoresist, which can be expressed as: Resolution 3 ×LER2×sensitivity≈constant. To meet the requirements of advanced photolithography, the main challenge of chemical amplification technology is to improve resolution and sensitivity while ensuring low LER. KrF photoresist mainly consists of four components: polymer resin, photosensitive agent, photosensitive base, and solvent. Existing photoresists and film-forming resins have the following problems that need to be solved: 1) The volatilization and diffusion of PAG and photoacid lead to reduced photoresist resolution and T-top phenomenon in photoresist morphology; 2) Linear polymers have large molecular weights and are prone to molecular chain entanglement, which leads to reduced photoresist resolution and increased edge roughness LER; 3) The volume of polymers is much larger than that of PAG small molecules. Chain entanglement and grain boundary effects will cause structural defects and uneven resolution.

[0003] Most of the photoresist film-forming polymer resins are linear structures. The linear polymer molecular structure prepared by free radical polymerization is large and dense, with a large molecular weight and a wide molecular weight distribution. Different molecular weights will lead to reduced photoresist resolution due to different dissolution rates. If there are fewer acid-sensitive groups in the molecular chain, the sensitivity of the photoresist will be reduced; molecular chain entanglement will lead to reduced photoresist resolution and LER performance. Summary of the invention

[0004] In order to solve the technical problems in the exposure and development of photoresist in the prior art, the present invention provides a KrF photoresist and a preparation method and a patterning method thereof.

[0005] In a first aspect, the present invention provides a KrF photoresist, which comprises, by weight percentage, 48.5-60.5% of a hyperbranched photoacid polymerized resin, 0.5-1% of a quencher, 0.03-0.5% of a leveling agent, and 50%-72% of a solvent;

[0006] The hyperbranched photoacid polymerized resin includes a hyperbranched ionic photoacid polymerized resin and a nonionic photoacid polymerized resin;

[0007] The hyperbranched photoacid polymerized resin is prepared by hyperbranched polymerization of polyol, p-hydroxystyrene monomer, alkenyl tert-butyl ester and photoacid monomer;

[0008] Furthermore, the hyperbranched photoacid polymerized resin can also be prepared by hyperbranched polymerization of polyol, hydroxystyrene monomer, alkenyl tert-butyl ester, photoacid monomer, and 4-(1-phenyl-1-hydroxyethyl)styrene;

[0009] Preferably, the 4-(1-phenyl-1-hydroxyethyl)styrene is hyperbranched polymerized after forming a polymer of p-hydroxystyrene monomer, alkenyl tert-butyl ester and photoacid monomer.

[0010] Preferably, the alkenyl tert-butyl ester is at least one of tert-butyl acrylate and tert-butyl crotonate.

[0011] Preferably, the photoacid monomer includes an ionic photoacid monomer and a non-ionic photoacid monomer, the ionic photoacid monomer is at least one of a triarylsulfonium monomer and a diaryliodonium monomer, and the non-ionic photoacid monomer is an N-sulfonyldicarboximide monomer (PIT).

[0012] Furthermore, the terminal group of the hyperbranched photoacid polymerized resin is a mercapto group.

[0013] Preferably, the quencher is an organic amine, which is at least one of trioctylamine, diethylamine, triethylamine, di-n-propylamine, and tri-2-(2-methoxy(ethoxy)ethylamine).

[0014] Preferably, the solvent is at least one of propylene glycol methyl ether acetate (PGMEA) or propylene glycol methyl ether (PGME).

[0015] Preferably, the molecular weight of the hyperbranched photoacid polymerized resin is 7500-50000, and the Tg value of the formed KrF photoresist is 123.5° C.-139.6° C.

[0016] In a second aspect, the present invention provides a method for preparing a KrF photoresist:

[0017] S100: Preparation of photoacid monomers

[0018] (1) Preparation of nonionic photoacid monomers

[0019] Dissolve sodium vinylbenzenesulfonate in DMF aqueous solution, disperse by ultrasonic wave, add thionyl chloride solution dropwise to obtain the intermediate product vinylbenzenesulfonyl chloride, dissolve the obtained vinylbenzenesulfonyl chloride in pyridine and acetonitrile, add N-hydroxyphthalimide, and fully react to obtain the non-ionic photoacid monomer;

[0020] (2) Preparation of ionic photoacid monomers

[0021] Sodium p-vinylbenzene sulfonate is dissolved in a DMF aqueous solution, dispersed by ultrasonication, and a diaryl iodonium salt or triaryl sulfonium salt aqueous solution is added dropwise to fully react to obtain an ionic photoacid monomer.

[0022] S200: Preparation of hyperbranched photoacid polymerized resin

[0023] The polyol and ethyl 2-[bis(2-hydroxyethyl)amino]acetate are dissolved in acetone solvent, dispersed by ultrasonic wave, reacted fully, and 60%-70% of p-hydroxystyrene monomer, 25-35% of alkenyl tert-butyl ester, and 5-10% of the non-ionic photoacid monomer prepared in step S100 or the ionic photoacid monomer prepared in step S200 are added respectively by weight ratio, stirred evenly, an initiator is added, an oil bath is carried out, reacted fully, thioglycolic acid is added for grafting modification, and an organic solvent is added for dilution to prepare a hyperbranched photoacid polymerized resin.

[0024] Furthermore, another preparation method is provided, wherein after adding an initiator, conducting an oil bath, and allowing sufficient reaction, 4-(1-phenyl-1-hydroxyethyl)styrene dissolved in an acetone solution is added, conducting an oil bath, and adding thioglycolic acid for grafting modification, and after sufficient reaction, a hyperbranched photoacid polymerized resin is obtained.

[0025] S300: Preparation of KrF photoresist

[0026] The prepared hyperbranched photoacid polymerized resin is dissolved in propylene glycol methyl ether acetate (PGMEA) or propylene glycol methyl ether (PGME) solvent according to weight percentage, and a quencher and a leveling agent are fully mixed to prepare a KrF photoresist.

[0027] In a third aspect, the present invention provides a KrF photoresist patterning method:

[0028] (1) providing a silicon-based substrate, baking at high temperature, spin coating a prepared KrF photoresist, and pre-baking to form a first glue layer;

[0029] (2) secondary spin coating, coating a photoresist based on linear poly(p-hydroxystyrene), secondary pre-baking, forming a second adhesive layer, and adjusting the relative thickness of the first adhesive layer and the second adhesive layer according to the undercut failure rate level;

[0030] (3) Exposure with a KrF excimer laser light source, post-baking, and development to form a pattern layer.

[0031] The beneficial effects achieved by the present invention are:

[0032] (1) Since the volatilization and diffusion of PAG and photoacid lead to the reduction of photoresist resolution and the appearance of T-top defects in photoresist morphology, the present invention builds a chain structure through hyperbranching, grafts and polymerizes 4-(1-phenyl-1-hydroxyethyl)styrene with phenyl groups at the tail end of the chain, and polymerizes the groups of the photoacid inside the chain, thereby encapsulating the groups of the photoacid, reducing the diffusion of the proton acid generated by the groups of the photoacid to the non-exposed area, and improving the resolution;

[0033] (2) By forming a chain-like resin structure, molecular chain entanglement is reduced, thereby improving the photoresist resolution and LER performance;

[0034] (3) By forming a chain-like resin structure, molecular chain entanglement is reduced and the Tg value is lowered;

[0035] (4) By polymerizing the photoacid groups in a hyperbranched chain structure, the proton acid inside the encapsulated structure can significantly improve the reaction efficiency, reduce the exposure energy, and improve the sensitivity and contrast of the KrF photoresist;

[0036] (5) When the alkenyl tert-butyl ester group is placed in the hyperbranched photoacid polymerized resin, the alkenyl tert-butyl ester group forms a carboxylic acid group after decomposition, which can inhibit the side reaction in the t-BOC deprotection, that is, the tert-butyl cation undergoes O-alkylation and C-alkylation with the resin in the t-BOC deprotection.

[0037] (6) The prior art uses acetoxy groups to hydrolyze under acid and alkali conditions to generate phenolic hydroxyl groups, and polymerizes acetoxystyrene to enhance the phenolic hydroxyl content, thereby improving the photoresist sensitivity and adhesion, and adjusting the photoresist retention rate, thereby avoiding side reactions in t-BOC deprotection. The present invention grafts 4-(1-phenyl-1-hydroxyethyl)styrene, and 4-(1-phenyl-1-hydroxyethyl)styrene is photoacid hydrolyzed to form alkenyl groups, which can also improve adhesion. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 This is the DSC test data diagram of Example 1;

[0040] Figure 2 It is a sensitivity test data diagram of an embodiment;

[0041] Figure 3 This is a photoresist development undercut yield test data diagram for the embodiment. DETAILED DESCRIPTION

[0042] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described below in conjunction with the accompanying drawings and embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0043] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0044] Embodiment 1: The present invention provides a method for preparing a KrF photoresist:

[0045] S100: Preparation of non-ionic photoacid monomers

[0046] Add 1 mol of sodium vinylbenzenesulfonate and 300 mL of DMF aqueous solution into a three-necked flask, disperse by ultrasonic, slowly drop 50 mL of thionyl chloride solution, stir magnetically for 30 min to fully react, let stand in a cold water bath for 12 h, add desiccant and ether, filter and evaporate to obtain vinylbenzenesulfonyl chloride.

[0047] Add the prepared vinylbenzenesulfonyl chloride into a three-necked flask and dissolve it in 0.55 mol of pyridine and 300 mL of acetonitrile. Add N-hydroxyphthalimide and react for 5-6 hours. Let stand for 30 minutes and dry to obtain N-sulfonyldicarboximide monomer.

[0048] S200: Preparation of ionic photoacid monomers

[0049] Take 1 mol of sodium p-vinylbenzenesulfonate and dissolve it in 300 mL of DMF aqueous solution, disperse it by ultrasonic for 30 min, slowly add 1 mol of triphenylsulfonium chloride aqueous solution, and continue the reaction for 3-5 hours.

[0050] S300: Preparation of hyperbranched photoacid polymerized resin

[0051] 1 mol of polyol (tetracycline) and 4 mol of ethyl 2-[bis(2-hydroxyethyl)amino]acetate were dissolved in a three-necked flask, 350 mL of acetone solvent was added, ultrasonic dispersion was performed, and the mixture was fully reacted for 1 h. 60%-70% of p-hydroxystyrene monomer, 25-35% of alkenyl tert-butyl ester, and 5-10% of the non-ionic photoacid monomer prepared in step S100 or the ionic photoacid monomer prepared in step S200 were added by weight, and the mixture was fully stirred. An initiator, azobisisobutyronitrile (AIBN), was added, and the mixture was fully reacted for 12 h in an oil bath at 65-75 degrees Celsius to obtain a viscous liquid. Thioglycolic acid was added for graft modification, acetone was added for dilution, and the mixture was dried to obtain a hyperbranched photoacid polymerized resin (without the addition of 4-(1-phenyl-1-hydroxyethyl)styrene).

[0052] After adding the initiator azobisisobutyronitrile (AIBN), the mixture was fully reacted for 10-12 hours in an oil bath at 65-75 degrees Celsius, 4-(1-phenyl-1-hydroxyethyl)styrene dissolved in acetone solution was added, the mixture was further heated to 65-75 degrees Celsius, thioglycolic acid was added for grafting modification, and the mixture was fully reacted for 2-3 hours to obtain a hyperbranched photoacid polymerized resin (with 4-(1-phenyl-1-hydroxyethyl)styrene added).

[0053] S300: Preparation of KrF photoresist

[0054] The prepared hyperbranched nonionic photoacid polymerized resin (without 4-(1-phenyl-1-hydroxyethyl)styrene), hyperbranched ionic photoacid polymerized resin (without 4-(1-phenyl-1-hydroxyethyl)styrene), hyperbranched ionic photoacid polymerized resin (with 4-(1-phenyl-1-hydroxyethyl)styrene), and hyperbranched ionic photoacid polymerized resin (with 4-(1-phenyl-1-hydroxyethyl)styrene) were dissolved in propylene glycol methyl ether acetate (PGMEA) or propylene glycol methyl ether (PGME) solvent, and tri-2-(2-methoxy(ethoxy)ethylamine) and leveling agent KP341 were fully mixed to prepare KrF photoresist.

[0055] Example 2: Photoresist DSC test

[0056] Take the same weight ratio of p-hydroxystyrene monomer, alkenyl tert-butyl ester and photoacid agent, mix them thoroughly, dissolve them in a solvent, add a leveling agent and an organic amine quencher, and prepare a photoresist based on linear poly-p-hydroxystyrene in the control test group. The four photoresists prepared in Example 1 are tested in parallel to test the corresponding glass transition temperatures. Figure 1 As shown:

[0057] From top to bottom, they are respectively the control group (photoresist based on linear poly(p-hydroxystyrene), hyperbranched ionic photoacid polymerized resin (with 4-(1-phenyl-1-hydroxyethyl)styrene added), hyperbranched ionic photoacid polymerized resin (with 4-(1-phenyl-1-hydroxyethyl)styrene added), hyperbranched non-ionic photoacid polymerized resin (without 4-(1-phenyl-1-hydroxyethyl)styrene added), and hyperbranched ionic photoacid polymerized resin (without 4-(1-phenyl-1-hydroxyethyl)styrene added).

[0058] Depend on Figure 1 It can be seen that the hyperbranched chain structures formed by the four polymer resins obtained in Example 1 have a lower glass transition temperature Tg than the linear structure. By forming a hyperbranched chain structure, the glass transition temperature is reduced by at least 27°C. This is mainly because the chain structure reduces the entanglement of the polymer. At the same time, the higher the degree of branching, the more active branching points there are, and more monomers will participate in the branching reaction, resulting in a shorter average molecular segment length of the polymer, a smaller molecular weight, and an increase in the internal free volume of the polymer, resulting in a lower Tg of the polymer.

[0059] At the same time, by Figure 1 It can be seen that adding 4-(1-phenyl-1-hydroxyethyl)styrene to the chain tail for hyperbranched polymerization increases the steric hindrance, and the glass transition temperature Tg is larger than that of the photoresist without adding 4-(1-phenyl-1-hydroxyethyl)styrene for hyperbranched polymerization.

[0060] Example 3: Sensitivity and contrast test

[0061] A control group (a photoresist based on linear poly(p-hydroxystyrene), PR1) and an experiment were set up: the hyperbranched ionic photoacid polymerized resin obtained in Example 1 (with 4-(1-phenyl-1-hydroxyethyl) styrene added, PR2), the hyperbranched ionic photoacid polymerized resin (with 4-(1-phenyl-1-hydroxyethyl) styrene added, PR3), the hyperbranched nonionic photoacid polymerized resin (without 4-(1-phenyl-1-hydroxyethyl) styrene added, PR4), and the hyperbranched ionic photoacid polymerized resin (without 4-(1-phenyl-1-hydroxyethyl) styrene added, PR5). The photoresists of the control group and the experimental group were spin-coated on a silicon-based substrate, film-coated, dried, exposed, dried, developed, and ion-implanted to obtain a pattern layer.

[0062] Depend on Figure 2 It can be seen that under the same light source conditions and exposure time, the sensitivity of the four hyperbranched photoacid polymerized resins is better than that of the control group. Among them, the exposure energy required for the resin in the experimental group without adding 4-(1-phenyl-1-hydroxyethyl)styrene for polymerization is less than the exposure energy required for adding 4-(1-phenyl-1-hydroxyethyl). This is because the thermal stability of tert-butyl ester mainly determines the required exposure energy. In the resins with the same mass fraction of polymerization, PR4 and PR5 have more tert-butyl acrylate added and stronger acid production capacity, while PR1 and PR2 have added 4-(1-phenyl-1-hydroxyethyl)styrene for polymerization. 4-(1-phenyl-1-hydroxyethyl)styrene is hydrolyzed under protonic acid, eliminates hydroxyl groups, and is converted into double bonds, and the overall acid production capacity is slightly weaker.

[0063] At the same time, it can be seen from Table 1 that the contrast of PR1 and PR2 is greater than that of PR4 and PR5. This is because 4-(1-phenyl-1-hydroxyethyl)styrene is polymerized at the tail of the chain segment. Due to the steric hindrance of the benzene ring, the proton acid fails to undergo a cross-linking reaction with the resin in the non-exposed area, which catalyzes the hydrolysis of 4-(1-phenyl-1-hydroxyethyl)styrene at the tail of the chain, reduces LER, and improves the contrast.

[0064]

[0065] Table 1

[0066] Example 4: Photoresist development undercut yield test

[0067] A silicon-based substrate is provided, high-temperature baked, and the KrF photoresist (PR2 or PR3) prepared in Example 1 is spin-coated and pre-baked to form a first glue layer; a second spin coating is performed to coat a photoresist based on linear poly(p-hydroxystyrene) and a second pre-baking is performed to form a second glue layer, and the relative thickness of the first glue layer and the second glue layer can be adjusted according to the undercut failure rate level; a KrF excimer laser light source is used for exposure, post-baking, and development is performed to form a pattern layer.

[0068] KrF photoresist is applied according to the relative thickness of the first glue layer and the second glue layer in a ratio of (0-2):1, such as Figure 3 By adjusting the relative thickness of the first glue layer and the second glue layer, the undercut failure rate can be optimized. When the relative thickness of the first glue layer and the second glue layer is in the range of (0.5-1):1, the undercut failure rate is reduced. Since the photoacidity of the substrates of the first glue layer and the second glue layer is different, setting a photoresist with strong photoacidity at the bottom of the glue layer can significantly reduce the undercut failure caused by insufficient exposure energy of the bottom glue layer or incomplete bonding and development with the substrate.

[0069] The photoresist prepared in this embodiment: 1) can reduce the reduction of photoresist resolution and the T-top defect in photoresist morphology caused by the volatilization and diffusion of PAG and photoacid; 2) at the same time, it reduces the entanglement of molecular chains, thereby improving the photoresist resolution and LER performance, and reducing the Tg value; 3) by polymerizing the photoacid groups in a hyperbranched chain structure, the proton acid inside the encapsulated structure can significantly improve the reaction efficiency, reduce the exposure energy, and improve the sensitivity and contrast of KrF photoresist.

[0070] Through the above specific implementations, those skilled in the art can easily implement the present invention. However, it should be understood that the present invention is not limited to the above specific implementations. On the basis of the disclosed implementations, those skilled in the art can arbitrarily combine different technical features to achieve different technical solutions.

Claims

1. A method for preparing a KrF photoresist, characterized in that: S100: Preparation of photoacid monomers (1) Preparation of non-ionic photoacid monomers Dissolving sodium vinylbenzenesulfonate in a DMF aqueous solution, dispersing by ultrasonication, and dropping a thionyl chloride solution to obtain an intermediate product, vinylbenzenesulfonyl chloride; dissolving the obtained vinylbenzenesulfonyl chloride in pyridine and acetonitrile, adding N-hydroxyphthalimide, and reacting sufficiently to obtain the nonionic photoacid monomer; (2) Preparation of ionic photoacid monomers Dissolve sodium p-vinylbenzene sulfonate in a DMF aqueous solution, disperse by ultrasonication, dropwise add a diaryl iodonium salt or a triaryl sulfonium salt aqueous solution, and react fully to obtain the ionic photoacid monomer; S200: Preparation of hyperbranched photoacid polymerized resin Dissolve the polyol and ethyl 2-[bis(2-hydroxyethyl)amino]acetate in acetone solvent, disperse by ultrasonic wave, fully react, add p-hydroxystyrene monomer, alkenyl tert-butyl ester, the non-ionic photoacid monomer or ionic photoacid monomer obtained in step S100 respectively by weight ratio, stir well, add initiator, and perform oil bath, after fully reacting, add 4-(1-phenyl-1-hydroxyethyl)styrene dissolved in acetone solution, perform oil bath, add thioglycolic acid for grafting modification, and after fully reacting, obtain the hyperbranched photoacid polymerized resin; S300: Preparation of KrF photoresist The hyperbranched photoacid polymerized resin is dissolved in propylene glycol methyl ether acetate (PGMEA) or propylene glycol methyl ether (PGME) solvent by weight percentage, and the quencher and leveling agent are fully mixed to obtain the KrF photoresist.