Preparation method, product and application of phosphogypsum-based concrete solid brick
By using phosphogypsum, blast furnace slag powder, cement and other materials to prepare high-strength phosphogypsum aggregate, the problem of aggregate substitution in concrete bricks is solved, efficient resource utilization of phosphogypsum is achieved, environmental pollution and resource waste are reduced, and it provides Efficient alternatives to building materials.
Patent Information
- Application Number
- CN202310574729.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-05-22
AI Technical Summary
Existing concrete bricks lack aggregate substitutes that can replace natural pebbles and gravel, and the utilization rate of phosphogypsum is low, resulting in environmental pollution and resource waste.
Phosphogypsum, blast furnace slag powder and cement are used as composite gel materials, supplemented by calcium oxide as an alkaline activator. By controlling the alkaline activator components, high-strength phosphogypsum aggregates are prepared, and based on them, Phosphogypsum-based concrete solid bricks that meet the requirements of concrete solid bricks simplify the aggregate preparation process and avoid the sintering process.
It achieves efficient resource utilization of phosphogypsum, reduces environmental pollution, improves the economic benefits of the phosphorus chemical industry, provides natural pebbles and gravel substitutes, meets the strength requirements of building materials, and promotes sustainable development.
Smart Images

Figure CN116553903B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of building materials, specifically to a preparation method, product and application of phosphogypsum-based concrete solid bricks. The present application uses phosphogypsum as the main raw material, successfully prepares high-strength phosphogypsum aggregate to replace natural pebbles and gravel, and successfully prepares corresponding concrete solid bricks, which is of great significance for solving the pollution problem of phosphogypsum and reducing the cost of building materials. Background Art
[0002] Phosphogypsum is a byproduct of the production process of phosphoric acid extraction by sulfuric acid method. It is also an industrial waste residue with calcium sulfate dihydrate as the main component. According to statistics, the cumulative global emission of phosphogypsum is about 6 billion tons, and it is increasing at a rate of 150 million tons / year. At present, the main method of treating phosphogypsum is open-air stacking. The large-scale storage of phosphogypsum not only occupies a large amount of land, but also pollutes groundwater, soil and atmosphere when stacked for a long time, destroys the surrounding ecological environment, and seriously hinders the sustainable development of the phosphorus chemical industry.
[0003] As a renewable resource with great potential, a lot of research has been carried out at home and abroad on phosphogypsum. Its main application areas include cement, gypsum building materials, roadbed and pavement engineering, chemical industry, agriculture (soil conditioner), etc. How to realize the resource utilization of phosphogypsum has always been a hot topic of research.
[0004] At present, the utilization of phosphogypsum in China is mainly concentrated in the building materials industry, industry and agriculture, among which the comprehensive application in the building materials industry accounts for the largest proportion. Using phosphogypsum, fly ash, quicklime and slag as raw materials, high-strength β-high-strength hemihydrate gypsum (MHG) is prepared after calcination. MHG can be used to prepare various building materials such as paper-faced gypsum boards to replace the consumption of natural gypsum. However, the key technical problem lies in the removal of impurities such as phosphorus and fluorine in phosphogypsum and the problem of crystal transformation.
[0005] On the other hand, concrete bricks have become a new type of building material to replace clay bricks. The raw materials for preparing concrete bricks include: cement, coarse and fine aggregates and admixtures. Commonly used coarse aggregates are pebbles and crushed stones, and commonly used fine aggregates are river sand and mountain sand. Natural sand and stone are non-renewable resources, which are obtained through mining. By destroying the ecological environment and obtaining natural crushed stones, river sand has been gradually banned and restricted.
[0006] In view of the lack of aggregates in concrete bricks, domestic and foreign research on the replacement of crushed stone aggregates in concrete has mostly focused on construction waste such as waste concrete and waste bricks. As early as after World War II, some developed countries in the world have carried out research on recycled concrete. Domestic universities such as Nanchang University and Wuhan University have also carried out research on the application of recycled aggregates in concrete.
[0007] Using phosphogypsum as a cement retarder instead of natural gypsum is an effective treatment method. Yu Wanzeng from Jilin University of Architecture used undisturbed phosphogypsum as a concrete additive. The results showed that phosphogypsum has a retarding and expansion effect on concrete and can stimulate the activity of mineral admixtures, but its optimal dosage in C30 concrete is only 3.0%~4.0%.
[0008] As mentioned above, existing concrete bricks lack aggregate substitutes that can replace natural pebbles and crushed stones, and phosphogypsum, as a construction waste, has a low utilization rate. Whether phosphogypsum can be used in the preparation of concrete bricks has become a technical problem that urgently needs to be solved. Summary of the invention
[0009] The purpose of the invention is to provide a preparation method, product and application of phosphogypsum-based concrete solid bricks in view of the above-mentioned existing problems. This application uses phosphogypsum as the main raw material, blast furnace slag powder and cement as composite gel materials, and is supplemented with an alkaline activator mainly composed of calcium oxide. By controlling the components of the alkaline activator, high-strength phosphogypsum aggregates are successfully prepared, and based on the prepared phosphogypsum aggregates, concrete solid bricks that meet the requirements of "Concrete Solid Bricks" (GB / T21144-2007) are successfully prepared. This application does not require sintering to prepare aggregates, which can effectively simplify the aggregate preparation process. At the same time, this application has a simple process, a reasonable flow, and is easy to operate, and can meet the requirements of industrial preparation of concrete solid bricks. The main raw materials of this application, blast furnace slag powder and phosphogypsum, are all from industrial waste, which can realize the resource utilization of materials, and are of great significance for protecting the environment, reducing environmental pollution, and achieving sustainable development.
[0010] In order to achieve the above object, the present invention adopts the following technical solution:
[0011] A method for preparing phosphogypsum-based concrete solid bricks comprises the following steps:
[0012] (1) Weigh the raw materials according to the following weight ratios: 100 parts of cement, 65-75 parts of water, and 600-750 parts of aggregate;
[0013] (2) Mix the weighed components evenly to form a slurry;
[0014] (3) After the slurry is extruded and formed, it is cured to obtain a phosphogypsum-based concrete solid brick;
[0015] In the step 1, the aggregate includes fine sand and phosphogypsum aggregate;
[0016] The weight ratio of the fine sand to the phosphogypsum aggregate is 1:1.9-2.2.
[0017] The particle size of the fine sand is in the range of 0.15 to 0.50 mm.
[0018] The particle size of the phosphogypsum aggregate is ≥4.75mm.
[0019] The particle size range of the phosphogypsum aggregate is 4.75~20mm.
[0020] The phosphogypsum aggregate is prepared by a method comprising the following steps:
[0021] (a) drying the phosphogypsum to obtain dried phosphogypsum;
[0022] (b) weighing powders of each component according to a ratio, mixing and stirring the weighed powders of each component to form a first intermediate;
[0023] (c) placing the prepared first intermediate into a mold of a pressure gauge for pressing, and compacting the mixture into a block, which is recorded as a second intermediate;
[0024] (d) mechanically crushing the second intermediate obtained in step c to form a coarse aggregate, which is recorded as a third intermediate;
[0025] (e) sieving the third intermediate to obtain aggregate blanks with different particle sizes;
[0026] (f) curing the aggregate blank obtained in step e at room temperature and a humidity of ≥70%; after the curing is completed, phosphogypsum aggregate is obtained;
[0027] In the step b, the mass percentage of each component is as follows: 55-65wt% phosphogypsum, 20-30wt% slag powder, 8-10wt% formed cement, 0.5-1.5wt% calcium oxide, 1.5-2.5wt% ammonium sulfate, 1.5-2.5wt% sodium silicate, and 1-3wt% cationic starch.
[0028] In the step a, the water content of the dried phosphogypsum is ≤5wt%.
[0029] The mass ratio of ammonium sulfate to sodium silicate is 1:0.9-1.2.
[0030] The molding cement is po42.5.
[0031] In the step f, the room temperature is 5-40° C., and the curing time is 1 d to 10 d.
[0032] The product prepared by the above-mentioned method for preparing phosphogypsum-based concrete solid bricks.
[0033] Application of the aforementioned phosphogypsum-based concrete solid bricks.
[0034] The phosphogypsum-based concrete solid brick is used as a building material.
[0035] The phosphogypsum-based concrete solid brick is used for wall production.
[0036] The phosphogypsum-based concrete solid brick is used for making non-load-bearing walls.
[0037] In response to the aforementioned problems, the present application provides a preparation method, product and application of phosphogypsum-based concrete solid bricks.
[0038] In the present application, the phosphogypsum aggregate is prepared from raw materials including the following components: phosphogypsum, slag powder, formed cement, calcium oxide, ammonium sulfate, sodium silicate, and cationic starch. Among them, phosphogypsum is used as the main raw material, blast furnace slag powder and cement are used as composite gel materials (blast furnace slag powder is based on steel slag and is a secondary waste product), supplemented with an alkaline activator mainly composed of calcium oxide, and high-strength phosphogypsum aggregate is successfully prepared by controlling the alkaline activator components.
[0039] Under normal conditions, slag powder contains a large amount of glass. After contact with water, the weakest Ca-O bond in the glass breaks, and the alkaline activator increases the pH value of the solution, accelerating the dissociation of Si-O and Al-O structures in the glass, generating silicate ions and aluminate ions, which react with the Ca2+ ions released by the slag hydrolysis. 2+ Reaction to generate hydrated calcium silicate and tricalcium aluminate; tricalcium aluminate reacts with gypsum to generate hydraulic ettringite; in addition, slag hydration produces hydrated calcium silicate gel (CSH gel). A small amount of hydraulic ettringite can fill the pores to reduce the shrinkage of the system and has almost no effect on the strength, but too much alkali activator will generate more hydraulic ettringite, causing the system to expand and generate greater internal stress, and then the strength will decrease with the increase of alkali activator. The structure of hydraulic ettringite will be destroyed under the evaporation of water over a long period of time, thereby reducing the strength.
[0040] In the present application, a method of controlling the amount of calcium oxide added and doping part of the cationic starch is adopted. When preparing the phosphogypsum aggregate, the components are evenly mixed together, and the cationic starch is evenly coated on the phosphogypsum. When the aggregate blank is prepared and cured in a high humidity environment, the phosphogypsum dissolves sulfate anions in water, which will adsorb with the cationic starch of the coating layer, thereby preventing the sulfate ions from hydrating with cement to form calcium sulfate. It should be noted that the present application does not use an external heat source to gelatinize the cationic starch, but gelatinizes the cationic starch based on the heat generated by the pyrolysis of calcium oxide in a high humidity environment. In this way, not only can the heat consumption required for heating and gelatinization be reduced, but also after gelatinization, mixing will cause the uniformity of the material to deteriorate, making the overall strength of the prepared phosphogypsum aggregate unstable. Based on the improved method, the problem of uneven mixing of phosphogypsum aggregate raw materials is solved, the energy consumption is reduced, and it is gelatinized after obtaining the aggregate blank, and the prepared phosphogypsum aggregate has higher strength and more stability. At the same time, the present application is doped with part of ammonium sulfate and sodium silicate; on the one hand, ammonium sulfate, sodium silicate and calcium oxide jointly act as stimulators; on the other hand, the test results show that there is an obvious synergistic effect between ammonium sulfate, sodium silicate, calcium oxide and components such as phosphogypsum and slag powder, which can effectively solidify calcium ions, inhibit the further dissolution of phosphogypsum in water, and improve the strength of phosphogypsum aggregate.
[0041] Based on the improved scheme, the phosphogypsum content in the phosphogypsum aggregate of the present application is greater than 40%, and the compressive strength of the phosphogypsum aggregate is greater than the strength of the diagenetic rock (not less than 30MPa). Furthermore, the present application successfully avoids the purification process of phosphogypsum, avoids the pollution of the environment by harmful components in phosphogypsum, and has a high utilization rate of phosphogypsum, which opens up a new way for phosphogypsum emission enterprises to comprehensively utilize phosphogypsum.
[0042] At the same time, the strength of concrete mainly depends on three aspects: the strength of cement stone, the strength of coarse aggregate, and the strength of the interface between coarse aggregate and cement stone matrix. For a long time, people have been focusing on the hydration of cement, concrete admixtures and mineral admixtures to improve the strength of concrete solid bricks, while ignoring the role of aggregates. Related studies have shown that under medium and strong matrix conditions, the strength of concrete increases with the increase of aggregate strength. In this application, high-strength phosphogypsum aggregates were successfully prepared, and the prepared phosphogypsum aggregates replaced natural pebbles and crushed stones to successfully prepare concrete solid bricks. The performance of the prepared phosphogypsum aggregate concrete hollow bricks meets the requirements of "Concrete Solid Bricks" (GB / T 21144-2007). The use of the present invention will help solve the problem of shortage of natural pebbles in my country and will be conducive to the promotion of corresponding environmental protection work.
[0043] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0044] (1) In the present application, the raw materials used for the preparation of phosphogypsum aggregate are cheap and sintering is not required, so the manufacturing cost of phosphogypsum aggregate is low; at the same time, the large-scale application of phosphogypsum (phosphogypsum dosage>40%) can not only reduce the waste disposal cost of the phosphorus chemical industry, but also increase the added value generated by the phosphorus chemical industry, and has broad market prospects;
[0045] (2) The adoption of this application can effectively solve the problem of resource utilization of phosphogypsum, open up a new way for resource utilization of phosphogypsum, and meet the requirements of circular economy and resource conservation and comprehensive utilization;
[0046] (3) The phosphogypsum aggregate of the present application is made into corresponding particle sizes according to the standard of "Pebbles and Crushed Stones for Construction" (GB / T14685-2011), and can be used as a substitute for pebbles or crushed stones, effectively solving the problem of shortage of natural pebbles and crushed stones, and has a positive effect on protecting the environment and improving the economic benefits of the phosphorus chemical industry;
[0047] (4) This application uses phosphogypsum aggregate as raw material and prepares concrete solid bricks in accordance with JGJ51-2002 "Technical Specification for Lightweight Aggregate Concrete". The prepared concrete solid bricks meet the requirements of "Concrete Solid Bricks" (GB / T21144-2007) (with a maximum strength of MU40) and can be used as a new type of building material;
[0048] (5) This application uses waste or secondary waste as the main raw material. The raw material cost is low and environmentally friendly. It can effectively reduce the damage to the environment caused by the construction industry and realize the resource utilization of materials. It is of great significance to protecting the environment, reducing environmental pollution and achieving sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] The present invention will now be described by way of example with reference to the accompanying drawings, in which:
[0050] Figure 1 This is a process flow chart for preparing phosphogypsum aggregate for this application. DETAILED DESCRIPTION
[0051] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any manner.
[0052] Any feature disclosed in this specification, unless otherwise stated, can be replaced by other equivalent or alternative features with similar purposes. That is, unless otherwise stated, each feature is only an example of a series of equivalent or similar features.
[0053] In the examples of this application, phosphogypsum (PG) was purchased from a place in Sichuan and is in the form of a gray powder, the main component of which is CaSO4•2H2O. 42.5 Ordinary Portland cement was purchased from a place in Sichuan; sodium silicate pentahydrate (AR), ammonium sulfate (AR), and quicklime (AR) were purchased from a company in Tianjin. Blast furnace slag powder is a commercially available product, and its activity index detection method complies with the national standard GB / T18046-2008. The product characteristics are: specific surface area 480-580m 2 / kg, physical appearance is spherical; activity index 3d ≥ 90%, 7d ≥ 100%, 28d ≥ 110%; fluidity ratio ≥ 100%, water content (mass fraction) ≤ 1.0%, sulfur trioxide (mass fraction) ≤ 4.0%, chloride ion (mass fraction) ≤ 0.06%, loss on ignition (mass fraction) ≤ 3.0%.
[0054] PG and PO42.5 cements were tested respectively, and their chemical compositions are shown in Table 1 below.
[0055] Table 1 Chemical composition
[0056] raw materials CaO / % <![CDATA[SO3 / %]]> SrO / % <![CDATA[SiO2 / %]]> <![CDATA[Al2O3 / %]]> <![CDATA[Fe2O3 / %]]> <![CDATA[P2O5 / %]]> <![CDATA[R2O / %]]> PG 30.85 31.85 - 4.65 4.2 - 3.22 0.32 PO 42.5 cement 65.34 4.63 - 19.43 4.88 1.2 0.04 0.27 raw materials <![CDATA[TiO2 / %]]> MgO / % BaO / % MnO / % ZnO / % <![CDATA[Zr2O / %]]> Cl / % PG 0.2 0.24 - - - - - PO 42.5 cement 0.06 0.61 0.43 - 0.02 0.02 0.04
[0057] Note: In Table 1, R2O represents an alkali metal oxide.
[0058] In this embodiment, since the phosphogypsum sample used is in the form of gray powder and has been dried, the corresponding drying step is omitted. In this embodiment, the curing temperature is 20-25°C; for ease of comparison, the curing time of all embodiments is 2 days, and the humidity of the curing box is 80-90%. After the curing of the phosphogypsum aggregate to be prepared is completed, the compressive strength at 3 days, 7 days, and 28 days is tested respectively.
[0059] Example 1
[0060] The process of preparing phosphogypsum aggregate in this embodiment is as follows.
[0061] (1) Weigh the raw materials
[0062] Weigh the components according to the proportion: 62% phosphogypsum, 25wt% slag powder, 10wt% PO42.5 cement, 1wt% calcium oxide, 2wt% cationic starch. Mix and stir the weighed components to obtain a first intermediate.
[0063] (2) Pressing
[0064] The prepared first intermediate is placed in a mold of a pressure gauge for pressing, and the mixture is compacted into a block, which is recorded as the second intermediate.
[0065] (3) Crushing
[0066] The obtained second intermediate is mechanically crushed to form a coarse aggregate, which is recorded as the third intermediate.
[0067] (4) Screening
[0068] The obtained third intermediate is sieved to obtain aggregate blanks with different particle sizes.
[0069] (5) Maintenance
[0070] The obtained aggregate blank is cured in a curing box at room temperature and 80-90% humidity. After the curing is completed, phosphogypsum aggregate is obtained.
[0071] Example 2
[0072] The process of preparing phosphogypsum aggregate in this embodiment is as follows.
[0073] (1) Weigh the raw materials
[0074] Weigh the components according to the proportion: 61% phosphogypsum, 25wt% slag powder, 10wt% PO42.5 cement, 2wt% calcium oxide, and 2wt% cationic starch. Mix and stir the weighed components to obtain a first intermediate.
[0075] (2) Pressing
[0076] The prepared first intermediate is placed in a mold of a pressure gauge for pressing, and the mixture is compacted into a block, which is recorded as the second intermediate.
[0077] (3) Crushing
[0078] The obtained second intermediate is mechanically crushed to form a coarse aggregate, which is recorded as the third intermediate.
[0079] (4) Screening
[0080] The obtained third intermediate is sieved to obtain aggregate blanks with different particle sizes.
[0081] (5) Maintenance
[0082] The obtained aggregate blank is cured in a curing box at room temperature and 80-90% humidity. After the curing is completed, phosphogypsum aggregate is obtained.
[0083] Example 3
[0084] The process of preparing phosphogypsum aggregate in this embodiment is as follows.
[0085] (1) Weigh the raw materials
[0086] Weigh the components according to the proportion: 62% phosphogypsum, 25wt% slag powder, 10wt% PO42.5 cement, 1wt% ammonium sulfate, 2wt% cationic starch. Mix and stir the weighed components to obtain a first intermediate.
[0087] (2) Pressing
[0088] The prepared first intermediate is placed in a mold of a pressure gauge for pressing, and the mixture is compacted into a block, which is recorded as the second intermediate.
[0089] (3) Crushing
[0090] The obtained second intermediate is mechanically crushed to form a coarse aggregate, which is recorded as the third intermediate.
[0091] (4) Screening
[0092] The obtained third intermediate is sieved to obtain aggregate blanks with different particle sizes.
[0093] (5) Maintenance
[0094] The obtained aggregate blank is cured in a curing box at room temperature and 80-90% humidity. After the curing is completed, phosphogypsum aggregate is obtained.
[0095] Example 4
[0096] The process of preparing phosphogypsum aggregate in this embodiment is as follows.
[0097] (1) Weigh the raw materials
[0098] Weigh the components according to the proportion: 60% phosphogypsum, 25wt% slag powder, 10wt% PO42.5 cement, 3wt% ammonium sulfate, 2wt% cationic starch. Mix and stir the weighed components to obtain a first intermediate.
[0099] (2) Pressing
[0100] The prepared first intermediate is placed in a mold of a pressure gauge for pressing, and the mixture is compacted into a block, which is recorded as the second intermediate.
[0101] (3) Crushing
[0102] The obtained second intermediate is mechanically crushed to form a coarse aggregate, which is recorded as the third intermediate.
[0103] (4) Screening
[0104] The obtained third intermediate is sieved to obtain aggregate blanks with different particle sizes.
[0105] (5) Maintenance
[0106] The obtained aggregate blank is cured in a curing box at room temperature and 80-90% humidity. After the curing is completed, phosphogypsum aggregate is obtained.
[0107] Example 5
[0108] The process of preparing phosphogypsum aggregate in this embodiment is as follows.
[0109] (1) Weigh the raw materials
[0110] Weigh the components according to the proportion: 62% phosphogypsum, 25wt% slag powder, 10wt% PO42.5 cement, 1wt% sodium silicate, 2wt% cationic starch. Mix and stir the weighed components to obtain a first intermediate.
[0111] (2) Pressing
[0112] The prepared first intermediate is placed in a mold of a pressure gauge for pressing, and the mixture is compacted into a block, which is recorded as the second intermediate.
[0113] (3) Crushing
[0114] The obtained second intermediate is mechanically crushed to form a coarse aggregate, which is recorded as the third intermediate.
[0115] (4) Screening
[0116] The obtained third intermediate is sieved to obtain aggregate blanks with different particle sizes.
[0117] (5) Maintenance
[0118] The obtained aggregate blank is cured in a curing box at room temperature and 80-90% humidity. After the curing is completed, phosphogypsum aggregate is obtained.
[0119] Example 6
[0120] The process of preparing phosphogypsum aggregate in this embodiment is as follows.
[0121] (1) Weigh the raw materials
[0122] Weigh the components according to the proportion: 60% phosphogypsum, 25wt% slag powder, 10wt% PO42.5 cement, 3wt% sodium silicate, 2wt% cationic starch. Mix and stir the weighed components to obtain a first intermediate.
[0123] (2) Pressing
[0124] The prepared first intermediate is placed in a mold of a pressure gauge for pressing, and the mixture is compacted into a block, which is recorded as the second intermediate.
[0125] (3) Crushing
[0126] The obtained second intermediate is mechanically crushed to form a coarse aggregate, which is recorded as the third intermediate.
[0127] (4) Screening
[0128] The obtained third intermediate is sieved to obtain aggregate blanks with different particle sizes.
[0129] (5) Maintenance
[0130] The obtained aggregate blank is cured in a curing box at room temperature and 80-90% humidity. After the curing is completed, phosphogypsum aggregate is obtained.
[0131] Example 7
[0132] The process of preparing phosphogypsum aggregate in this embodiment is as follows.
[0133] (1) Weigh the raw materials
[0134] Weigh the components according to the proportion: 61% phosphogypsum, 25wt% slag powder, 10wt% PO42.5 cement, 1wt% calcium oxide, 1wt% ammonium sulfate, 2wt% cationic starch. Mix and stir the weighed components to obtain a first intermediate.
[0135] (2) Pressing
[0136] The prepared first intermediate is placed in a mold of a pressure gauge for pressing, and the mixture is compacted into a block, which is recorded as the second intermediate.
[0137] (3) Crushing
[0138] The obtained second intermediate is mechanically crushed to form a coarse aggregate, which is recorded as the third intermediate.
[0139] (4) Screening
[0140] The obtained third intermediate is sieved to obtain aggregate blanks with different particle sizes.
[0141] (5) Maintenance
[0142] The obtained aggregate blank is cured in a curing box at room temperature and 80-90% humidity. After the curing is completed, phosphogypsum aggregate is obtained.
[0143] Example 8
[0144] The process of preparing phosphogypsum aggregate in this embodiment is as follows.
[0145] (1) Weigh the raw materials
[0146] Weigh the components according to the proportion: 60% phosphogypsum, 25wt% slag powder, 8wt% PO42.5 cement, 1wt% calcium oxide, 2wt% ammonium sulfate, 2wt% sodium silicate, 2wt% cationic starch. Mix and stir the weighed components to obtain a first intermediate.
[0147] (2) Pressing
[0148] The prepared first intermediate is placed in a mold of a pressure gauge for pressing, and the mixture is compacted into a block, which is recorded as the second intermediate.
[0149] (3) Crushing
[0150] The obtained second intermediate is mechanically crushed to form a coarse aggregate, which is recorded as the third intermediate.
[0151] (4) Screening
[0152] The obtained third intermediate is sieved to obtain aggregate blanks with different particle sizes.
[0153] (5) Maintenance
[0154] The obtained aggregate blank is cured in a curing box at room temperature and 80-90% humidity. After the curing is completed, phosphogypsum aggregate is obtained.
[0155] Example 9
[0156] The process of preparing phosphogypsum aggregate in this embodiment is as follows.
[0157] (1) Weigh the raw materials
[0158] Weigh the components according to the proportion: 61% phosphogypsum, 25wt% slag powder, 8wt% PO42.5 cement, 1wt% calcium oxide, 1.5wt% ammonium sulfate, 1.5wt% sodium silicate, 2wt% cationic starch. Mix and stir the weighed components to obtain a first intermediate.
[0159] (2) Pressing
[0160] The prepared first intermediate is placed in a mold of a pressure gauge for pressing, and the mixture is compacted into a block, which is recorded as the second intermediate.
[0161] (3) Crushing
[0162] The obtained second intermediate is mechanically crushed to form a coarse aggregate, which is recorded as the third intermediate.
[0163] (4) Screening
[0164] The obtained third intermediate is sieved to obtain aggregate blanks with different particle sizes.
[0165] (5) Maintenance
[0166] The obtained aggregate blank is cured in a curing box at room temperature and 80-90% humidity. After the curing is completed, phosphogypsum aggregate is obtained.
[0167] Example 10
[0168] The process of preparing phosphogypsum aggregate in this embodiment is as follows.
[0169] (1) Weigh the raw materials
[0170] Weigh the components according to the proportion: 55% phosphogypsum, 28.5wt% slag powder, 9wt% PO42.5 cement, 1wt% calcium oxide, 2wt% ammonium sulfate, 2wt% sodium silicate, 2.5wt% cationic starch. Mix and stir the weighed components to obtain a first intermediate.
[0171] (2) Pressing
[0172] The prepared first intermediate is placed in a mold of a pressure gauge for pressing, and the mixture is compacted into a block, which is recorded as the second intermediate.
[0173] (3) Crushing
[0174] The obtained second intermediate is mechanically crushed to form a coarse aggregate, which is recorded as the third intermediate.
[0175] (4) Screening
[0176] The obtained third intermediate is sieved to obtain aggregate blanks with different particle sizes.
[0177] (5) Maintenance
[0178] The obtained aggregate blank is cured in a curing box at room temperature and 80-90% humidity. After the curing is completed, phosphogypsum aggregate is obtained.
[0179] The properties of the phosphogypsum aggregates prepared in Examples 1 to 10 above were tested, and the results are shown in Table 2.
[0180] Table 2 Compressive strength test results of phosphogypsum aggregate
[0181]
[0182] Embodiment 11
[0183] The phosphogypsum aggregates prepared in Examples 8, 9, and 10 were used as raw materials (corresponding to sequence numbers 1, 2, and 3 in Table 3, respectively) to prepare concrete solid bricks, and the relevant information is shown in Table 3 below.
[0184] Table 3 Material ratio and compressive strength
[0185] Serial number PO42.5 cement / kg Water / kg Fine sand / kg Phosphogypsum aggregate / kg 28d compressive strength / MPa 1 100 70 275 555 42.2 2 100 70 275 555 42.4 3 100 70 275 555 44.1
[0186] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a phosphogypsum-based concrete solid brick, characterized in that: The steps include: (1) Weigh the raw materials according to the following weight ratios: 100 parts of cement, 65-75 parts of water, and 600-750 parts of aggregate; (2) Mix the weighed components evenly to form a slurry; (3) After the slurry is extruded and formed, it is cured to obtain a phosphogypsum-based concrete solid brick; In the step 1, the aggregate includes fine sand and phosphogypsum aggregate; The weight ratio of the fine sand to the phosphogypsum aggregate is 1:1.9-2.2; The phosphogypsum aggregate is prepared by a method comprising the following steps: (a) drying the phosphogypsum to obtain dried phosphogypsum; (b) weighing powders of each component according to a ratio, mixing and stirring the weighed powders of each component to form a first intermediate; (c) placing the prepared first intermediate into a mold of a pressure gauge for pressing, and compacting the mixture into a block, which is recorded as a second intermediate; (d) mechanically crushing the second intermediate obtained in step (c) to form a coarse aggregate, which is recorded as a third intermediate; (e) sieving the third intermediate to obtain aggregate blanks with different particle sizes; (f) curing the aggregate blank obtained in step (e) at room temperature and a humidity of ≥70%; after the curing is completed, phosphogypsum aggregate is obtained; In the step (b), the mass percentage of each component is as follows: 55-65wt% phosphogypsum, 20-30wt% slag powder, 8-10wt% formed cement, 0.5-1.5wt% calcium oxide, 1.5-2.5wt% ammonium sulfate, 1.5-2.5wt% sodium silicate, and 1-3wt% cationic starch.
2. The method for preparing phosphogypsum-based concrete solid brick according to claim 1, characterized in that: In the step (a), the moisture content of the dried phosphogypsum is ≤5wt%.
3. The method for preparing phosphogypsum-based concrete solid brick according to claim 1, characterized in that: The mass ratio of ammonium sulfate to sodium silicate is 1:0.9-1.
2.
4. The method for preparing the phosphogypsum-based concrete solid brick according to any one of claims 1 to 3, characterized in that: In the step (f), the room temperature is 5-40° C. and the curing time is 1 d to 10 d.
5. The product prepared by the method for preparing phosphogypsum-based concrete solid bricks according to any one of claims 1 to 4.
6. Use of the phosphogypsum-based concrete solid bricks as claimed in claim 5.
7. The use according to claim 6, characterized in that: The phosphogypsum-based concrete solid brick is used as a building material.
8. The use according to claim 7, characterized in that: The phosphogypsum-based concrete solid brick is used for wall production.
9. The use according to claim 8, characterized in that: The phosphogypsum-based concrete solid brick is used for making non-load-bearing walls.
Citation Information
Cited By
Method for preparing mesoporous silica and co-producing calcium sulfate whisker from manganese slag and / or phosphogypsum, mesoporous silica and application thereof
CN122484928A