A high-strength, high-ductility hydrogen embrittlement-resistant medium-entropy alloy and a preparation method thereof

CN116574958BActive Publication Date: 2024-11-05SHANGHAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310262420.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-11-05
Estimated Expiration
2043-03-17

AI Technical Summary

Technical Problem

[0008]可以看到,现有技术中合金成分复杂,难以兼顾材料强度和塑性,而且合金制作工艺操作步骤复杂、耗时长、成本高

Benefits of technology

[0024] The invention also provides a high-strength, high-ductility hydrogen embrittlement-resistant medium-entropy alloy prepared by the preparation method. The chemical formula of the high-strength, high-ductility hydrogen embrittlement-resistant medium-entropy alloy is (FeCrNi) 100-x B x , the molar ratio of Fe, Cr, and Ni in the chemical formula is equal, and x is defined as above. The high-strength, high-ductility hydrogen embrittlement-resistant medium-entropy alloy is composed of FCC phase and has a cellular substructure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116574958B_ABST
    Figure CN116574958B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-strength, high-ductility hydrogen embrittlement resistant medium entropy alloy and a preparation method thereof. The preparation method comprises: according to the chemical formula (FeCrNi) 100‑x B x The Fe, Cr, Ni particles and FeB powder of corresponding masses are weighed respectively, the FeB powder is pressed into a disc-shaped block, the raw materials are dried, and then put into an arc melting furnace to melt and obtain an alloy ingot; in the chemical formula, the molar ratio of Fe, Cr, Ni is equal, x represents the molar ratio, and x=1-4; the obtained alloy ingot is heat treated at 1000-1200°C, kept warm for 1.5-2.5 hours, and quenched after the end of the heat preservation; then several forgings are performed, and the process of each forging is as follows: uniform forging is performed after heating and softening at 1000-1200°C, and quenching is performed after the forging is completed; finally, annealing treatment is performed at 1000-1200°C, kept warm for 1.5-2.5 hours, and quenching is performed after the heat preservation is completed, so as to obtain a high-strength, high-ductility hydrogen embrittlement-resistant medium-entropy alloy with a cellular substructure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new materials, and in particular to a high-strength, high-ductility hydrogen embrittlement-resistant medium-entropy alloy and a preparation method thereof. Background Art

[0002] The development of metal materials has a profound impact on the production level of human society. With the high-quality development of productivity, especially in aerospace, deep-sea exploration, new energy and other fields, higher requirements are also placed on the performance of metal materials.

[0003] Traditional alloys are mainly composed of one or two elements, while high-entropy alloys break the design concept of traditional alloys. High-entropy alloys are new alloys composed of five or more main elements, and their mixing entropy is greater than 1.5R, where R is the molar gas constant 8.314J / (mol·K). Compared with traditional alloy materials, high-entropy alloys have four major characteristics: high-entropy effect, lattice distortion, slow diffusion and cocktail effect. Therefore, high-entropy alloys show better mechanical properties, corrosion resistance, and oxidation resistance. With the development of high-entropy alloys in the past 20 years, medium-entropy alloys with simpler preparation processes, easier composition control, and better performance have gradually been developed on their basis. Medium-entropy alloys are alloys composed of two to four main elements, and their mixing entropy is greater than 1.0R and less than 1.5R.

[0004] Hydrogen embrittlement now refers to the entry of hydrogen atoms from the environment into the interior of the material. When hydrogen accumulates inside the material and exceeds the critical concentration, it will have a catastrophic effect on the performance of the material, especially in metal materials. Hydrogen embrittlement can easily cause the failure of metal materials.

[0005] In recent years, many studies have found that high (medium) entropy alloys have great potential in hydrogen embrittlement resistance, such as CoCrFeMnNi high entropy alloys and CoCrNi medium entropy alloys. However, due to the high price of Co, these alloys are difficult to apply in the large-scale market. Therefore, selecting a Co-free alloy that is resistant to hydrogen embrittlement is of great significance in practical applications.

[0006] Zhang Jian et al. (Effect of grain boundary phase on hydrogen embrittlement of Fe-Ni-Cr austenitic alloy, Acta Metallurgica Sinica, Vol. 44, No. 9, September 2008, pp. 1095-1098) studied the internal friction behavior of two Fe-Ni-Cr austenitic alloys containing boron (B) and without boron, and found that B weakened the ability of grain boundaries to capture hydrogen by inhibiting the precipitation of grain boundary phases, thereby reducing hydrogen-induced plastic loss. In this study, the alloy composition is complex and the process is time-consuming. After smelting and forging, it is necessary to undergo hot rolling, 980℃ solid solution for 1h, water quenching, 740℃ aging for 32h and air cooling. In addition, the alloy 2 containing 0.008wt% B during the smelting process requires a higher smelting temperature and significantly longer time than the alloy 1 without B. In addition, this study did not explore the effect of B doping on the mechanical properties of the alloy.

[0007] The patent specification with publication number CN 102409258 A discloses a boron-containing high-strength, hydrogen-embrittlement-resistant alloy and a method for controlling its microstructure uniformity. The boron content of the boron-containing alloy in the patented technology is 0.001wt% to 0.1wt%, and its microstructure uniformity control method still requires hot rolling, solution treatment, water quenching and aging treatment, and different solution heat treatments are required according to the change of boron content.

[0008] It can be seen that the alloy composition in the prior art is complex, and it is difficult to balance the strength and plasticity of the material. In addition, the alloy manufacturing process has complicated operation steps, is time-consuming, and has high costs. Therefore, there is an urgent need for a method that can easily prepare high-boron content alloys to facilitate large-scale production of high-strength, high-ductility, hydrogen embrittlement-resistant medium-entropy alloys. Summary of the invention

[0009] In view of the above technical problems and the deficiencies in the art, the present invention provides a method for preparing a high-strength, high-ductility hydrogen embrittlement-resistant medium-entropy alloy, which has low cost and simple preparation process, and obtains (FeCrNi) with relatively ideal mechanical properties and hydrogen embrittlement resistance. 100-x B x Medium entropy alloy. The present invention uses FeB (CAS No. 12006-84-7) powder as a boron source, and significantly increases the amount of B added by regulating the content of each added element and the ratio between them, further improving the alloy's hydrogen embrittlement resistance, and effectively improving the alloy's mechanical properties. The present invention selects appropriate smelting technical parameters and optimizes the heat treatment process to obtain (FeCrNi) with uniform composition, high density, and cellular substructure. 100-x B x Medium entropy alloy resistant to hydrogen embrittlement.

[0010] The specific technical solutions are as follows:

[0011] A method for preparing a high-strength, high-ductility hydrogen embrittlement-resistant medium-entropy alloy, comprising:

[0012] Step 1: According to the chemical formula (FeCrNi) 100-x B x The ratio of the four elements is converted, and the corresponding masses of Fe, Cr, Ni particles and FeB powder are weighed respectively, and the FeB powder is pressed into a disc-shaped block using a powder tablet press, and these raw materials are dried and then placed in an arc melting furnace to melt and obtain an alloy ingot; in the chemical formula, the molar ratio of Fe, Cr, Ni, etc. is to obtain a better combination of strength and ductility, x represents the molar ratio, x=1-4 (corresponding to a B content of about 0.2wt% or more), preferably, x=1.5-2, and the anti-hydrogen embrittlement effect can be best;

[0013] Step 2: heat-treating the alloy ingot obtained in step 1 at 1000-1200° C. for 1.5-2.5 hours, and then quenching the alloy ingot after the heat-treating.

[0014] Step 3, subjecting the alloy ingot quenched in step 2 to forging treatment for several times, wherein the process of each forging treatment is as follows: heating at 1000-1200° C. to soften and then uniformly forging, and then quenching treatment is performed after forging is completed;

[0015] Step 4: annealing the alloy block after forging in step 3 at 1000-1200° C. for 1.5-2.5 hours, and quenching after the insulation to obtain a high-strength, high-ductility, hydrogen embrittlement-resistant medium-entropy alloy with a cellular substructure.

[0016] Preferably, in step 1, the mass purity of Fe, Cr, Ni particles and FeB powder is greater than 99.8%.

[0017] Preferably, in step 1, the temperature of the drying treatment is 50-120°C.

[0018] Further preferably, in step 1, the drying process is carried out in a vacuum drying oven, the temperature of the vacuum drying oven is 100° C., and the drying time is 2 hours.

[0019] Preferably, in step one, the order of the piles placed in the arc melting furnace from bottom to top is Ni, Fe, FeB, and Cr, the melting atmosphere is high-purity argon with a purity of not less than 99.99%, and the gas pressure is 0.005 to 0.015 MPa higher than the atmospheric pressure, and the arc striking current is 120 to 320 A.

[0020] Preferably, in step 1, the metal ingot is repeatedly turned over more than 3 times during smelting to ensure that the composition of the metal ingot is uniform.

[0021] Preferably, in step 2, the heat treatment is carried out in a muffle furnace.

[0022] Preferably, in step three, a total of 3 to 6 forging processes are performed.

[0023] Preferably, in step 4, the annealing treatment is carried out in a muffle furnace.

[0024] The present invention also provides a high-strength, high-ductility, hydrogen embrittlement-resistant medium-entropy alloy prepared by the preparation method. The chemical formula of the high-strength, high-ductility, hydrogen embrittlement-resistant medium-entropy alloy is (FeCrNi) 100-x B x , where Fe, Cr, Ni have the same molar ratio in the chemical formula, and x is defined as above. The high-strength, high-ductility hydrogen embrittlement-resistant medium-entropy alloy is composed of an FCC phase and has a cellular substructure.

[0025] The high-strength, high-ductility hydrogen embrittlement-resistant medium-entropy alloy of the present invention has a tensile strength greater than 600 MPa and a tensile ductility greater than 30%. After hydrogen charging, the tensile strength is greater than 590 MPa, the tensile ductility is greater than 22%, and the hydrogen embrittlement factor is less than 35%.

[0026] The present invention provides a method for preparing high-strength and high-ductility (FeCrNi) 100-x B x The process parameters of the medium entropy alloy resistant to hydrogen embrittlement are controlled by controlling the composition ratio and preparation process of the medium entropy alloy to obtain (FeCrNi) with low cost, simple process, good hydrogen embrittlement resistance, excellent mechanical properties and cellular substructure. 100-x B x Medium entropy alloy.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1. The present invention effectively improves the microstructure of the medium entropy alloy by regulating the hot working process and the atomic ratio of elements, thereby simultaneously improving the plasticity and strength of the alloy.

[0029] 2. The present invention effectively increases the doping amount of B by using FeB as a boron source, and further effectively improves the mechanical properties of the medium-entropy alloy by regulating the atomic ratio of the doped B element, while also improving the hydrogen embrittlement resistance of the medium-entropy alloy, making it suitable for aerospace, deep-sea exploration, new energy and other fields.

[0030] 3. Medium-entropy alloy (FeCrNi) provided by the present invention 100-x B xNot only does it simplify the alloy composition, but it also obtains excellent strength and plasticity at the same time, overcoming the problem that the alloy composition of the prior art is complex and it is difficult to balance the strength and plasticity of the material. The medium entropy alloy of the present invention is a high-boron medium entropy alloy of pure FCC phase, forming a cellular substructure. At the same time, the medium entropy alloy is prepared by an arc melting method, and only needs to undergo heat treatment-forging-annealing treatment. The process flow is simple and takes only about 3-5 hours, overcoming the problems of complex operation steps, long time consumption, and high cost in the alloy manufacturing process of the prior art. The medium entropy alloy of the present invention has uniform composition and low raw material cost, which is of great value to the industrial application of medium entropy alloys. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 X-ray diffraction (XRD) diagram of the medium-entropy alloy prepared in Example 4-7.

[0032] Figure 2 This is a metallographic micrograph of the FeCrNi medium-entropy alloy prepared in Example 4 of the present invention.

[0033] Figure 3 (FeCrNi) prepared in Example 5 of the present invention 99 Metallographic micrograph of B1 medium entropy alloy.

[0034] Figure 4 (FeCrNi) prepared in Example 6 of the present invention 98.5 B 1.5 Metallographic micrograph of medium entropy alloy.

[0035] Figure 5 (FeCrNi) prepared in Example 7 of the present invention 98 Metallographic micrograph of B2 medium entropy alloy. DETAILED DESCRIPTION

[0036] The present invention will be further described below in conjunction with the accompanying drawings and specific examples. It should be understood that these examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. The operating methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0037] Example 1

[0038] The chemical formula of the medium entropy alloy prepared in this embodiment is: Fe 40 Cr 20 Ni 40 .

[0039] The entropy alloy preparation process in this embodiment is as follows:

[0040] Step 1: According to Fe 40 Cr 20 Ni 40The atomic ratio of each element of the medium entropy alloy is converted into the mass ratio of each component, and Fe, Cr, and Ni particles with a mass purity greater than 99.8% are used for batching. The weighed raw materials are placed in a vacuum drying oven and dried at 100°C for 2h;

[0041] Step 2: Place a total of 100 g of material into a water-cooled copper crucible of a high-throughput arc melting furnace in the order of Ni, Fe, and Cr from bottom to top, and evacuate the high-throughput arc melting furnace to 1×10 -3 Pa, and then introduce argon gas to make the melting atmosphere high-purity argon gas with a purity of not less than 99.99%, and the gas pressure is 0.005-0.015MPa higher than the atmospheric pressure;

[0042] Step 3: preheat the raw materials with an arc current of 120A, and gradually adjust the current from 120A to 120-320A. After the smelting is completed, wait for the alloy to cool, turn the alloy over and repeat the above smelting process; after the first turning over, the intermediate alloy is initially formed, and the intermediate alloy is turned over 3 times, and arc smelting is carried out with a current of 280A to make the alloy composition uniform. After the smelting is completed, wait for the sample to cool for 20 minutes to form an alloy ingot, and open the furnace to take out the alloy ingot;

[0043] Step 5: Place the alloy ingot in a muffle furnace, heat to 1100°C and keep warm for 2 hours, then quickly quench and cool;

[0044] Step 6: Place the alloy ingot after the treatment in step 5 into a forging furnace at 1100°C and heat it until the alloy ingot softens. Take it out with a clamp and evenly forge the surface of the alloy ingot. Repeat the forging three times and place it in cooling water to cool it down. Forge the alloy ingot into a long strip forging.

[0045] Step 7: Place the long strip forging in step 6 into a muffle furnace, heat to 1100° C. and keep warm for 2 hours, then quickly quench and cool to form the final medium entropy alloy;

[0046] Step 8, the medium entropy alloy prepared in step 7 is made into a tensile specimen, and the tensile specimen is ground with SiC sandpaper to remove surface scratches and oxide layer;

[0047] Step 9: Under room temperature conditions, use a universal testing machine to perform a slow tensile test on the tensile specimen in step 8 at a tensile rate of 0.001 / s to test the yield strength, tensile strength and elongation of the sample.

[0048] Example 2

[0049] The chemical formula of the medium entropy alloy prepared in this embodiment is: Fe 40 Cr 40 Ni 20 .

[0050] The entropy alloy preparation process in this embodiment is the same as that in embodiment 1. The only difference is that in step 1, Fe 40 Cr 40 Ni 20 The atomic ratio of each element of the medium entropy alloy is converted into the mass ratio of each component by using Fe, Cr and Ni particles with a mass purity greater than 99.8% for batching.

[0051] Example 3

[0052] The chemical formula of the medium entropy alloy prepared in this embodiment is: Fe 20 Cr 40 Ni 40 .

[0053] The entropy alloy preparation process in this embodiment is the same as that in embodiment 1. The only difference is that in step 1, Fe 20 Cr 40 Ni 40 The atomic ratio of each element of the medium entropy alloy is converted into the mass ratio of each component by using Fe, Cr and Ni particles with a mass purity greater than 99.8% for batching.

[0054] Example 4

[0055] The chemical formula of the medium entropy alloy prepared in this embodiment is: FeCrNi.

[0056] The entropy alloy preparation process in this embodiment is the same as that in Embodiment 1, except that in step 1, Fe, Cr, and Ni particles with a mass purity greater than 99.8% are used for batching according to the atomic ratio of each element of the entropy alloy in FeCrNi converted into the mass ratio of each component.

[0057] This embodiment also conducts a hydrogen charging experiment. Specifically, the tensile specimen in step eight is taken and hydrogen is charged using an electrochemical cathode hydrogen charging method. A 10 mm × 10 mm platinum electrode is used as the anode and the tensile specimen is used as the cathode. The electrolyte is an aqueous solution of 0.5 M sulfuric acid + 2 g / L thiourea. The hydrogen charging time is 2 hours and the current density is 10 mA / cm 2 Then, a slow tensile test is performed on the hydrogen-filled tensile specimen according to the method of step nine to test the yield strength, tensile strength and elongation of the hydrogen-filled specimen.

[0058] The phase structure of the entropy alloy in this embodiment was characterized using an X-ray diffractometer. The results are shown in Figure 1 The microstructure of the entropy alloy in this embodiment was observed using a metallographic microscope. Figure 2 .

[0059] Table 1 shows the test results of Examples 1-4.

[0060] Table 1

[0061]

[0062] It can be seen from the above examples 1 to 4 that the FeCrNi isoatomic ratio medium entropy alloy provided by the present invention has a good combination of strength and ductility, and its tensile strength is significantly better than that of Fe 40 Cr 20 Ni 40 , Fe 20 Cr 40 Ni 40 , its ductility is significantly better than Fe 40 Cr 40 Ni 20 .

[0063] Example 5

[0064] The chemical formula of the medium entropy alloy prepared in this embodiment is: (FeCrNi) 99 B1.

[0065] The entropy alloy preparation process and test process in this embodiment are the same as those in Example 4, except that step 1 is carried out according to (FeCrNi) 99 The atomic ratio of each element in the entropy alloy in B1 is converted into the mass ratio of each component, and Fe, Cr, Ni particles and FeB powder with a mass purity greater than 99.8% are used for mixing, wherein FeB powder is used as a boron source, and the FeB powder is pressed into a disc-shaped block using a powder tablet press with a tablet pressing pressure of 40kN. In step 2, a total of 100g of material is placed in a water-cooled copper crucible of a high-throughput arc melting furnace in the order of Ni, Fe, FeB, and Cr from bottom to top.

[0066] The phase structure of the entropy alloy in this embodiment was characterized using an X-ray diffractometer. The results are shown in Figure 1 The microstructure of the entropy alloy in this embodiment was observed using a metallographic microscope. Figure 3 .

[0067] Example 6

[0068] The chemical formula of the medium entropy alloy prepared in this embodiment is: (FeCrNi) 98.5 B 1.5 .

[0069] The entropy alloy preparation process and test process in this embodiment are the same as those in Example 5, except that step 1 is carried out according to (FeCrNi) 98.5 B 1.5 The atomic ratio of each element of the medium entropy alloy is converted into the mass ratio of each component by using Fe, Cr, Ni particles and FeB powder with a mass purity greater than 99.8% for mixing.

[0070] The phase structure of the entropy alloy in this embodiment was characterized using an X-ray diffractometer. The results are shown in Figure 1 The microstructure of the entropy alloy in this embodiment was observed using a metallographic microscope. Figure 4 .

[0071] Example 7

[0072] The chemical formula of the medium entropy alloy prepared in this embodiment is: (FeCrNi) 98 B2.

[0073] The entropy alloy preparation process and test process in this embodiment are the same as those in Example 5, except that step 1 is carried out according to (FeCrNi) 98 The atomic ratio of each element in the entropy alloy B2 is converted into the mass ratio of each component and the Fe, Cr, Ni particles and FeB powder with a mass purity greater than 99.8% are used for mixing.

[0074] The phase structure of the entropy alloy in this embodiment was characterized using an X-ray diffractometer. The results are shown in Figure 1 The microstructure of the entropy alloy in this embodiment was observed using a metallographic microscope. Figure 5 .

[0075] XRD phase analysis was performed on the medium-entropy alloys of Examples 4 to 7, and it was found that the medium-entropy alloys of Examples 4 to 7 were all single FCC phase.

[0076] The metallographic analysis of the medium entropy alloys of Examples 4 to 7 revealed that (FeCrNi) prepared in Examples 5 to 7 99 B1, (FeCrNi) 98.5 B 1.5 、(FeCrNi) 98 Compared with the FeCrNi medium entropy alloy prepared in Example 4, the B2 medium entropy alloy has a cellular substructure.

[0077] The mechanical properties of the medium entropy alloys of Examples 4 to 7 were tested, and their yield strength, tensile strength, ductility and hydrogen embrittlement factor (percentage of ductility loss after hydrogen charging) are shown in Table 2 below.

[0078] Table 2

[0079]

[0080] Note: The smaller the hydrogen embrittlement factor, the stronger the hydrogen embrittlement resistance of the medium entropy alloy.

[0081] It can be seen from the above Examples 4 to 7 that the (FeCrNi) 100-x B x Compared with FeCrNi medium entropy alloy, hydrogen embrittlement resistant medium entropy alloy has better mechanical properties and good hydrogen embrittlement resistance.

[0082] In addition, it should be understood that after reading the above description of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A method for preparing a high-strength, high-ductility hydrogen embrittlement-resistant medium-entropy alloy, characterized in that: include: Step 1: According to the chemical formula (FeCrNi) 100-x B x The ratio of the four elements is converted, and the corresponding masses of Fe, Cr, Ni particles and FeB powder are weighed respectively, and the FeB powder is pressed into a disc-shaped block using a powder tablet press, and these raw materials are dried and then put into an arc melting furnace to melt and obtain an alloy ingot; in the chemical formula, the molar ratio of Fe, Cr, Ni, etc., x represents the molar ratio, and x=1-4; Step 2: heat-treating the alloy ingot obtained in step 1 at 1000-1200° C. for 1.5-2.5 hours, and then quenching the alloy ingot after the heat-treating. Step 3, subjecting the alloy ingot quenched in step 2 to forging treatment for several times, wherein the process of each forging treatment is as follows: heating at 1000-1200° C. to soften and then uniformly forging, and then quenching treatment is performed after forging is completed; Step 4: annealing the alloy block after forging in step 3 at 1000-1200° C. for 1.5-2.5 hours, and quenching after the insulation to obtain a pure FCC medium entropy alloy with high strength and high elongation and cellular substructure that resists hydrogen embrittlement.

2. The preparation method according to claim 1, characterized in that: In the chemical formula, x=1.5-2.

3. The preparation method according to claim 1, characterized in that: In step 1, the mass purity of Fe, Cr, Ni particles and FeB powder is greater than 99.8%.

4. The preparation method according to claim 1, characterized in that: In step 1, the temperature of the drying treatment is 50-120°C.

5. The preparation method according to claim 1, characterized in that: In step 1, the order of the piles placed in the arc melting furnace from bottom to top is Ni, Fe, FeB, and Cr. The melting atmosphere is high-purity argon with a purity of not less than 99.99%, and the gas pressure is 0.005 to 0.015 MPa higher than the atmospheric pressure. The arc striking current is 120 to 320A.

6. The preparation method according to claim 1, characterized in that: In step 1, the metal ingot is repeatedly turned over more than 3 times during smelting.

7. The preparation method according to claim 1, characterized in that: In step three, a total of 3 to 6 forging processes are performed.

8. The high-strength, high-ductility hydrogen embrittlement-resistant medium-entropy alloy prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The chemical formula of the high-strength, high-ductility hydrogen embrittlement-resistant medium-entropy alloy is (FeCrNi) 100-x B x , composed of FCC phase and has a cellular substructure.