A method for controlling corner crack defects in ship plate steel ingots

By controlling the cooling rate at the corners of the billet shell, installing anti-radiation insulation covers and multi-point continuous straightening technology, the problem of corner cracks in ship plate steel billets has been solved, the quality of the billet and production stability have been improved, and it is suitable for packaging Crystal steel products.

CN116586578BActive Publication Date: 2024-10-22ANGANG STEEL CO LTD
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
CN202310280960.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-22
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

Corner transverse cracks often occur in ship plate steel slabs during the continuous casting process. It is difficult to fundamentally solve this problem with existing technology, which affects the quality of the slabs.

Method used

By controlling the cooling rate of the billet shell corners in the mold, the cooling rate of the billet from the sector-shaped section to the corners before flame cutting, and the billet straightening method, a cooling method that combines slow cooling and rapid cooling is adopted, and Anti-radiation insulation covers are installed at the corners, combined with multi-point continuous straightening technology, to control the temperature of the corners of the slab.

Benefits of technology

It effectively avoids the occurrence and expansion of cracks at the corners of the cast slab, significantly improves the quality of the ship plate steel cast slab, and is suitable for peritectic steel products with simple process, low cost and strong adaptability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116586578B_ABST
    Figure CN116586578B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for controlling corner crack defects of ship plate steel ingots. The method is based on conventional production processes and achieves the purpose of controlling corner crack defects of ingots by comprehensive measures of controlling the temperature of the corner of the primary ingot shell in the crystallizer, the temperature of the corner from the sector to the front of flame cutting, and the straightening method of the ingots. The method can fundamentally solve the problem that corner crack defects are easily generated in the production process of ship plate steel ingots of peritectic steel, and can promote the stable production of defect-free ingots of ship plate steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron and steel metallurgy, and in particular relates to a method for controlling corner crack defects of ship plate steel ingots. Background Art

[0002] In the continuous casting production of microalloyed steel, peritectic and subperitectic steel slabs, transverse cracks in the corners have long been one of the problems that have plagued metallurgical workers at home and abroad. Although many literatures have conducted in-depth research on its generation mechanism and control measures, under the existing technical conditions, even world-leading companies such as Germany's Thyssen, Austria's Voestalpine, Japan's Nippon Steel, and South Korea's Posco cannot fundamentally solve it.

[0003] Ship plate steel (such as AH32, DH36) is a peritectic steel containing Nb and Ti microalloys. Since the C in the ship plate steel composition is in the peritectic steel range and contains microalloying elements Nb, V, and Ti that are prone to cracking, it is easy to have surface quality defects (corner crack defects) in the billet during continuous casting, and it is one of the more difficult steels to be continuously cast in continuous casting production. Many metallurgical producers have found that there are many reasons for the cracks in the billet, including casting equipment reasons, process operation factors, and the influence of solidification and cooling conditions. The mechanical behavior of the continuous casting billet during solidification at high temperature is also one of the most important influencing factors. These mechanical behaviors involve the strength limit, plastic deformation behavior, and thermal and mechanical stress of the continuous casting billet as the temperature decreases at high temperature. At high temperatures, when the stress on the billet exceeds the strain limit value at the corresponding temperature, the billet cracks will occur.

[0004] However, due to the differences in molten steel conditions, production equipment and technical levels of each ship plate steel manufacturer, the control measures and effects of the corner crack defects of ship plate steel ingots are also different. The measures currently taken cannot fundamentally solve this problem, and the impact of the corner crack defects on the quality of ship plate steel ingots is still a difficult problem that needs to be solved urgently.

[0005] The patent document with publication number CN105316558A discloses a method for preparing boron-containing steel for preventing corner cracking of ingots, which comprises pretreatment of molten iron, converter smelting, refining outside the furnace, continuous casting of steel billets, reheating of slabs and hot rolling in sequence. The composition of the boron-containing steel is as follows: C: 0.17-0.18, Si: 0.02-0.20, Mn: 0.23-1.26, P<0.017, S<0.014, N<0.0052, B: 0.0005-0.0010, Al: 0.015-0.034, and the balance is Fe. Ti is added in a mass percentage of 0.01-0.035 during the refining process outside the furnace. After adding titanium to the hot-rolled boron-added steel of the present invention, the quality of the ingots is significantly improved, and the off-line cleaning rate is reduced to 15.06%. Statistical results show that the defect rate has been reduced to 1.39%. In addition, the results of the test and analysis of the mechanical properties of boron-containing steel show that the mechanical properties of boron-containing steel are also improved after adding Ti. This invention adds titanium to the steel. Titanium mainly plays the role of fixing nitrogen. During the solidification process, Ti2N2 and Ti3N4 will first precipitate out of the molten steel, preventing the precipitation of BN. However, compared with traditional boron-containing steel, this invention needs to increase the coiling temperature and the final rolling temperature, and needs to combine the control of C in the steel and the production control of each process. It has poor adaptability to the complex production process on site and is difficult to control, so its application is limited.

[0006] The patent document with application publication number CN106475539A discloses a device and method for reducing corner cracks of ingots. The device consists of an electric control cabinet, an electromagnetic induction coil and a cooling device. The induction coil is first installed in the gap between two rollers before the ingot enters the straightening section, and the ingot is allowed to pass through the coil and connected to the cooling device; before continuous casting begins, the hollow copper tube in the electromagnetic induction coil is cooled by water; the conductivity of the cooling water is less than 50μs / cm; when the ingot pulling speed is 0.5-5m / min, the power of the electric control cabinet is turned on to supply power to the electromagnetic induction coil, and the electric control cabinet provides the electromagnetic induction coil with a medium frequency power supply with a frequency of 200-20000Hz and a rated power of 10kW-300kW; ensure that the corner temperature is higher than 1000℃ when the ingot enters the straightening section; after the continuous casting is completed, the power of the electric control cabinet is disconnected, and the hollow copper tube of the electromagnetic induction coil continues to be cooled by water until the ambient temperature is lower than 50℃ and the cooling water is disconnected. This invention uses electromagnetic induction heating to quickly promote the temperature rise of the corners of the ingot without contact and pollution, reduce the degree of defects in the corners of the ingot, alleviate the pressure of subsequent cleaning of the corners of the ingot, and improve the quality of the ingot. However, this process requires increased equipment and maintenance costs, and the heating and raising of the temperature control of the corners of the ingot is unstable and the effect is poor.

[0007] The patent document with the authorization announcement number CN208929147U discloses a synchronous solidification crystallizer, in which the guide water jacket of the crystallizer contacts and supports the four corners of the copper tube of the crystallizer. Since the guide water jacket is directly supported on the four corners of the copper tube of the crystallizer, the accuracy of the water seam of the crystallizer is greatly improved; at the same time, since the guide water jacket contacts the four corners of the copper tube of the crystallizer, the cooling of the corners of the copper tube of the crystallizer is weakened, so that the cooling intensity of the corners and the face of the copper tube of the crystallizer is uniform. The utility model has a simple structure and intuitive effect, and realizes synchronous solidification along the circumference of the crystallizer during the initial solidification of the continuous casting molten steel, reducing the tendency of the ingot to crack at the corner and de-square. However, the use cost or technical transformation cost of the invention is high, and the adaptability to metal grades and steel types is poor. Summary of the invention

[0008] The present invention provides a method for controlling the corner crack defect of a ship plate steel ingot. The method is based on a conventional production process and achieves the purpose of controlling the corner crack defect of the ingot by controlling the temperature of the corner of the primary ingot shell in the crystallizer, the temperature of the corner from the fan-shaped section of the ingot to the front of the flame cutting, and the ingot straightening method. The method can fundamentally solve the problem that corner crack defects are easily generated in the production process of peritectic steel ship plate steel ingots, and can promote the stable production of defect-free ingots of ship plate steel.

[0009] In order to achieve the above object, the present invention adopts the following technical solutions:

[0010] A method for controlling corner crack defects of ship plate steel ingots is based on conventional ship plate steel production processes, and controls the cooling rate of the ingot shell corners in the crystallizer, the cooling rate of the ingot from the fan-shaped section to the corners before flame cutting, and the ingot straightening method to achieve the effect of controlling the corner crack defects of the ingot, and specifically includes:

[0011] 1) Slow cooling method is adopted at the corner of the billet in the upper half of the crystallizer: 256m 3 / h≤Cooling water flow rate at wide corners≤320m 3 / h, 19.2m 3 / h≤ Cooling water flow rate at narrow corners≤24m 3 / h; Rapid cooling method is adopted at the corner of the billet in the lower half of the crystallizer: 352m 3 / h≤Cooling water flow rate at wide corners≤480m 3 / h、26.4m 3 / h≤ Cooling water flow rate at narrow corners≤36m 3 / h;

[0012] 2) Controlling the cooling rate of the billet from the fan-shaped section to the corner before flame cutting: installing an anti-radiation heat insulation cover at the corner of the billet, the anti-radiation heat insulation cover is composed of an outer metal layer (preferably a steel plate layer) and an inner refractory heat insulation layer, and the inner surface of the anti-radiation heat insulation cover is smooth;

[0013] 3) The billet straightening method adopts multi-point continuous straightening, and the billet corner temperature before straightening is ≥900℃;

[0014] The method is suitable for the production of high-grade ship plate steel with a carbon content of 0.10wt% to 0.17wt%.

[0015] The cross-sectional dimensions of the ingot are (170-200)×(1500-2000) mm.

[0016] Preferably, the anti-radiation heat-insulating covers are symmetrically arranged on both sides of the billet along the running track of the billet, and are arranged in a connected manner on the narrow surface of the billet and outside the upper and lower corners of the narrow surface.

[0017] Preferably, the anti-radiation heat-insulating cover is composed of two surfaces forming an angle, which are respectively arranged outside the four corners of the ingot and symmetrically arranged along the running track of the ingot.

[0018] The distance from the exit of the 1 / 2 sector segment to the front of the flame cutting is ≤ the length of the anti-radiation heat preservation cover ≤ the distance from the exit of the sector segment to the front of the flame cutting, and the angle of the anti-radiation heat preservation cover is 60°≤α≤90°.

[0019] For the ingot with a cross-sectional size of (170-200) × (1500-2000) mm, in conventional technology, the cooling method adopted at the corner of the ingot in the upper half of the crystallizer is the same as the cooling method adopted at the corner of the ingot in the lower half of the crystallizer: the wide surface cooling water flow rate is 320m 3 / h, cooling water flow rate at narrow corners is 24m 3 / h. The present invention adopts a slow cooling method at the corner of the billet in the upper half of the crystallizer, and the cooling water flow rate at the corner of the wide face and the cooling water flow rate at the corner of the narrow face are compared with the conventional cooling situation, and the cooling intensity is reduced by 0% to 20%; the corner of the billet in the lower half of the crystallizer adopts a fast cooling method, that is, the cooling intensity is increased by 10% to 50% under normal cooling conditions. The purpose of the design of the present invention is: the slow cooling method at the corner of the billet in the upper half of the crystallizer can make the temperature and thickness of the primary billet shell at the corner of the billet consistent with other parts, so as to achieve the purpose of synchronous solidification of the billet shell around the cross section of the billet, and at the same time avoid the high-temperature stress concentration caused by uneven solidification and shrinkage of the billet shell, resulting in the generation of crack sources of the billet edge crack; the fast cooling method at the corner of the billet in the lower half of the crystallizer can avoid or shorten the peritectic reaction time of ship plate steel, so that the atomic diffusion in the solid on which the peritectic reaction depends cannot be fully carried out, and the peritectic reaction is incomplete, resulting in a small linear shrinkage coefficient of steel, a small linear shrinkage of steel, and cracks are not easy to occur at the corner of the billet.

[0020] The present invention controls the cooling speed of the corners from the sector of the billet to the front of the flame cutting, and installs an anti-radiation heat-insulating cover at the corners of the billet. The purpose of this design is to install a heat-insulating cover at the corners of the billet from the sector of the billet to the front of the flame cutting, which can keep the corners of the billet warm and slow down the fast cooling speed of the corners due to two-dimensional heat transfer. At the same time, the length of the heat-insulating cover is set and the angle between the two sides is 60°≤α≤90°, and the inner surface of the heat-insulating cover is smooth, so that the radiant heat emitted by the billet during the whole process or at least half of the process from the crystallizer to the straightening can be reflected by the smooth inner surface of the heat-insulating cover, and the heat is reflected to the corners of the billet, which keeps the corners warm or even heats them, and avoids the billet from having too low a temperature at the corners before entering the straightening, which causes cracks in the billet during the straightening.

[0021] The present invention adopts multi-point continuous straightening to reduce the stress and strain at the corners of the ingot, reduce the strain rate in the straightening section, and avoid the occurrence of cracks at the corners of crack-sensitive steel grades. The temperature of the corners of the ingot before straightening is ≥900°C, which can avoid the third brittle temperature zone during steel solidification and reduce the occurrence of cracks.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The present invention effectively improves the corner temperature during the production of ship plate steel billet by controlling the cooling rate of the billet shell corner in the crystallizer, the cooling rate of the corner from the billet exiting the fan-shaped section to before flame cutting, and the billet straightening method, thereby avoiding the generation and expansion of corner cracks. The method for controlling the corner crack defects of ship plate steel billet of the present invention can achieve stable control of the corner crack defects of ship plate steel billet, and can also achieve stable control of the corner crack defects of peritectic steel billet steel that is prone to corner crack defects, which can significantly improve the quality of peritectic steel products such as ship plate steel, and the process is simple and the cost is low, so it is conducive to promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a structural schematic diagram of the anti-radiation heat preservation cover in the present invention in which one side is connected.

[0025] Figure 2 It is a schematic structural diagram of the arrangement of the external components of the anti-radiation heat preservation cover at the four corners of the ingot in the present invention.

[0026] In the figure: 1-outer steel plate layer, 2-inner refractory insulation layer, 3-cast billet, 4-anti-radiation insulation cover. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0028] Embodiment 1:

[0029] For AH32 ingots (C: 0.15%, cross-sectional dimensions 200×1950mm) produced by a certain factory, a slow cooling method is adopted at the corners of the upper half of the crystallizer (total length of the crystallizer is 900mm) during the continuous casting process: the cooling water flow rate at the wide corner is 304m 3 / h, narrow surface cooling water flow rate 22.8m 3 / h; Rapid cooling is adopted at the corners of the ingot in the lower half of the crystallizer: the cooling water flow rate at the wide corner is 384m 3 / h, cooling water flow rate at narrow corners: 28.8m 3 / h;

[0030] Anti-radiation heat preservation covers are installed at the corners of the ingot. The anti-radiation heat preservation covers are composed of an outer steel plate layer and an inner refractory heat preservation layer. The inner surface of the anti-radiation heat preservation covers is smooth. The anti-radiation heat preservation covers are symmetrically arranged on both sides of the ingot along the running track of the ingot, and are arranged in a connected manner on the narrow surface of the ingot and the outer sides of the upper and lower corners of the narrow surface (such as Figure 1 The length of the anti-radiation heat preservation cover is: the distance from the exit of the 1 / 2 sector segment to the front of the flame cutting, and the angle of the anti-radiation heat preservation cover is α=90°; the billet straightening method adopts multi-point continuous straightening, and the temperature of the billet corner is measured to be 905℃ before straightening.

[0031] After production, the dendrite samples of the continuous casting slab were taken for low-power inspection of the slab solidification structure and defective dendrite corrosion. The test results are shown in Table 1.

[0032] Table 1 Macroscopic inspection results of solidification structure and defective dendrite corrosion of ingot in Example 1

[0033]

[0034] After testing, the quality of the ingot is good and there are no corner cracks.

[0035] Embodiment 2:

[0036] For the ship plate steel DH36 ingot (C: 0.16%, cross-sectional dimensions 200×1950mm) produced by a certain factory, during the continuous casting process, a slow cooling method is adopted at the corner of the upper half of the crystallizer (total length of the crystallizer is 900mm): the cooling water flow rate at the wide corner is 288m 3 / h, cooling water flow rate at narrow corners: 21.6m 3 / h; Rapid cooling is adopted at the corners of the ingot in the lower half of the crystallizer: the cooling water flow rate at the wide corner is 432m 3 / h, cooling water flow rate at narrow corners: 32.4m 3 / h;

[0037] An anti-radiation heat preservation cover is installed at the corner of the billet. The anti-radiation heat preservation cover is composed of an outer steel plate layer and an inner refractory heat preservation layer. The inner surface of the anti-radiation heat preservation cover is smooth. The anti-radiation heat preservation cover is composed of two surfaces forming an angle and is respectively arranged outside the four corners of the billet, and is symmetrically arranged along the running track of the billet (such as Figure 2 The length of the anti-radiation heat preservation cover is: the distance from the fan-shaped segment outlet to the front of the flame cutting, the anti-radiation heat preservation cover angle α=80°, and the inner surface of the anti-radiation heat preservation cover is smooth; the billet straightening method adopts multi-point continuous straightening, and the temperature of the billet corner is measured to be 916℃ before straightening.

[0038] After production, the dendrite samples of the continuous casting slab were taken for low-power inspection of the slab solidification structure and defective dendrite corrosion. The test results are shown in Table 2.

[0039] Table 2 Low-power inspection results of solidification structure and defective dendrite corrosion of Example 2

[0040]

[0041] After testing, the quality of the ingot is good and there are no corner cracks.

[0042] Embodiment 3:

[0043] For the ship plate steel Q355B ingot (C: 0.16%, cross-sectional dimensions 200×1950mm) produced by a certain factory, during the continuous casting process, a slow cooling method is adopted at the corner of the upper half of the crystallizer (total length of the crystallizer is 900mm): the cooling water flow rate at the wide corner is 272m 3 / h, cooling water flow rate at narrow corners: 20.4m 3 / h; Rapid cooling is adopted at the corners of the ingot in the lower half of the crystallizer: the cooling water flow rate at the wide corner is 480m 3 / h, cooling water flow rate at narrow corners 36m 3 / h;

[0044] An anti-radiation heat preservation cover is installed at the corner of the billet. The anti-radiation heat preservation cover is composed of an outer steel plate layer and an inner refractory heat preservation layer. The inner surface of the anti-radiation heat preservation cover is smooth. The anti-radiation heat preservation cover is composed of two surfaces forming an angle and is respectively arranged outside the four corners of the billet, and is symmetrically arranged along the running track of the billet (such as Figure 2 The length of the anti-radiation heat preservation cover is: 0.8×the distance from the fan-shaped segment outlet to the front of the flame cutting, and the anti-radiation heat preservation cover angle α=75°; the billet straightening method adopts multi-point continuous straightening, and the temperature of the billet corner is measured to be 913℃ before straightening.

[0045] After production, the dendrite samples of the continuous casting slab were taken for low-power inspection of the slab solidification structure and defective dendrite corrosion. The test results are shown in Table 3;

[0046] Table 3 Low-power inspection results of solidification structure and defective dendrite corrosion of Example 3

[0047]

[0048] After testing, the quality of the ingot is good and there are no corner cracks.

[0049] In summary, the present invention can solve the problem of frequent corner transverse cracks in the ingot during the continuous casting process due to the special composition of ship plate steel (C is in the peritectic steel range), and is particularly suitable for the production of peritectic steel ingots such as ship plate steel.

Claims

1. A method for controlling corner crack defects in ship plate steel ingots, characterized in that: The method is based on the conventional production process of ship plate steel, and adopts the cooling rate of the corner of the shell of the ingot in the crystallizer, the cooling rate of the corner from the fan-shaped section of the ingot to the front of the flame cutting, and the ingot straightening method to achieve the effect of controlling the corner crack defect of the ingot, which specifically includes: 1) Slow cooling method is adopted at the corner of the billet in the upper half of the crystallizer: 256m 3 / h≤Cooling water flow rate at wide corners≤320m 3 / h, 19.2m 3 / h≤ Cooling water flow rate at narrow corners≤24m 3 / h; Rapid cooling method is adopted at the corner of the billet in the lower half of the crystallizer: 352m 3 / h≤Cooling water flow rate at wide corners≤480m 3 / h、26.4m 3 / h≤ Cooling water flow rate at narrow corners≤36m 3 / h; 2) Control the cooling speed from the billet exiting the fan-shaped section to the corner before flame cutting: install an anti-radiation heat preservation cover at the corner of the billet, the anti-radiation heat preservation cover is composed of an outer metal layer and an inner refractory heat preservation layer, and the inner surface of the anti-radiation heat preservation cover is smooth; 3) The ingot straightening method adopts multi-point continuous straightening, and the temperature of the ingot corner before straightening is ≥900℃.

2. The method for controlling corner crack defects of ship plate steel ingot according to claim 1, characterized in that: The method is suitable for the production of ship plate steel with a carbon content of 0.10wt% to 0.17wt%.

3. The method for controlling corner crack defects of ship plate steel ingot according to claim 1, characterized in that: The cross-sectional dimensions of the ingot are (170-200) × (1500-2000) mm.

4. The method for controlling corner crack defects of ship plate steel ingot according to claim 1, characterized in that: The anti-radiation heat-insulating covers are symmetrically arranged on both sides of the casting billet along the running track of the casting billet, and are arranged in a connected manner outside the narrow surface of the casting billet and the upper and lower corners of the narrow surface.

5. The method for controlling corner crack defects of ship plate steel ingot according to claim 1, characterized in that: The anti-radiation heat-insulating cover is composed of two surfaces forming an angle, which are respectively arranged outside the four corners of the casting billet and symmetrically arranged along the running track of the casting billet.

6. A method for controlling corner crack defects of ship plate steel ingot according to claim 5, characterized in that: The distance from the exit of the 1 / 2 sector segment to the front of the flame cutting is ≤ the length of the anti-radiation heat preservation cover ≤ the distance from the exit of the sector segment to the front of the flame cutting, and the angle of the anti-radiation heat preservation cover is 60°≤α≤90°.

Citation Information

Patent Citations

  • Preparation method of boron-containing steel preventing casting blank corner cracking

    CN105316558A

  • Device for alleviating corner cracks of casting blank and crack reduction method

    CN106475539A

  • Synchronous solidification crystallizer

    CN208929147U

  • Method for controlling the cross crack of blank angle of high nitrogen steel casting board containing vanadium

    CN101036939A

  • Device and method for reducing angle cracks of microalloyed plate blank

    CN106938324A