Arc welding rod for 1000MPa high-strength steel preheat-free welding and preparation method thereof
By designing arc welding rods with high strength, high toughness welding core and coating coating, the problems of moderate strong matching and cracks in welding of 1000MPa high-strength steel are solved, achieving high-strength, low-crack welding effects and simplifying the welding process.
Patent Information
- Application Number
- CN202310447985.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-04-24
AI Technical Summary
There is a lack of equal-strength matching electrode products during the welding process of 1000MPa high-strength steel, and the crack sensitivity of high-strength steel makes welding difficult and it is difficult to avoid cracks in the weld area.
Develop a 1000MPa high-strength steel preheat-free arc welding rod composed of a welding core and a coating skin. The welding core is composed of C, Si, Mn, Cr, Ni, Mo, etc. The coating skin contains nano-TiN powder. Through reasonable design of the welding core and The coating composition is used to prepare high-strength and high-toughness arc welding rods, which are pressed and dried using a spiral pressure coater to prepare the welding rods.
It achieves a welded joint strength of more than 1000MPa, a tensile strength of more than 1100MPa, and a -40°C impact energy of not less than 47J, avoiding cracks during room temperature welding, achieving equal-strength matching and no preheating welding, and simplifying operations.
Smart Images

Figure BDA0004196381180000051 
Figure BDA0004196381180000061
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal material welding, and in particular to an arc welding rod for preheat-free welding of 1000MPa high-strength steel and a preparation method thereof. Background Art
[0002] With the rapid development of the national economy, the trend of steel structure manufacturing towards large-scale development is becoming more and more obvious, and the strength grade of the steel used is getting higher and higher. In the technical fields of hydropower, engineering machinery, containers, large submersibles, etc., 1000MPa high-strength steel has begun to be used for design and manufacturing.
[0003] Due to its wide range of applications, arc welding is still the main welding method for 1000MPa high-strength steel. However, arc welding of high-strength steel has the following problems:
[0004] (1) 1000MPa high-strength steel and welding rods generally adopt low-strength matching, and there is no welding rod product that can match the same strength, which greatly limits the application of 1000MPa high-strength steel.
[0005] (2) High-strength steel has a high crack sensitivity, which brings great trouble to high-strength steel welding. Although with the advancement of metallurgical technology, cracks in the heat-affected zone of welding have rarely appeared, cracks in the weld zone are still difficult to avoid, and the weld zone has become the weakest area of the welded joint.
[0006] The present invention focuses on the welding application demand of 1000MPa high-strength steel and develops arc welding rods that are strongly matched with steel and can be welded without preheating. This is of great significance to improving the strength of steel used in large structures, making the manufacturing process green and environmentally friendly, and reducing the overall manufacturing cost. Summary of the invention
[0007] The present invention provides an arc welding rod for preheat-free welding of 1000MPa high-strength steel and a preparation method thereof. When the arc welding rod is used to weld 1000MPa high-strength steel, the strength of the welded joint is not less than 1000MPa, and no cracks are generated during room temperature welding. The problems of low toughness and insufficient strength of the welded joint during welding of 1000MPa-grade ultra-high-strength steel and cracking of the weld during welding are solved.
[0008] In order to achieve the above object, the present invention adopts the following technical solutions:
[0009] An arc welding rod for 1000MPa high-strength steel preheat-free welding, the arc welding rod comprising a welding core and a coating outer skin coated on the outside of the welding core; wherein the composition of the welding core is calculated by mass percentage as follows: C: 0.04%-0.08%, Si: 0.15%-0.35%, Mn: 1.85%-2.1%, Cr: 0.4%-0.6%, Ni: 4.5%-5.5%, Mo: 0.6%-0.9%, S≤0.008%, P≤0.010%, and the balance is iron; the composition of the coating outer skin is calculated by mass percentage as follows: CaCO 3 :24%~30%,SiO 2 :16%~21%,CaF 2 :18%~25%,TiO 2 : 10% ~ 15%, nano-TiN powder: 4% ~ 6.5%, and the rest is iron powder.
[0010] Furthermore, the average particle size of the nano-TiN powder is 20-45 nm.
[0011] A method for preparing an arc welding rod for preheat-free welding of 1000MPa high-strength steel comprises the following steps:
[0012] (1) Drawing the welding wire steel wire rod into a welding wire with a diameter of 3.2 to 4.0 mm;
[0013] (2) Using a welding wire of a set length as a welding core; adding a coating used as a coating outer skin to an adhesive and mixing them evenly; in terms of mass percentage, the amount of the adhesive added is 15% to 20% of the total amount of the coating;
[0014] (3) Pressing the welding core and the coating mixed with the adhesive into a welding rod;
[0015] (4) Dry the welding rod at 360-400℃ for more than 2h to obtain arc welding rod.
[0016] Furthermore, the length of the welding wire as the welding core is 350 to 400 mm.
[0017] Further, the adhesive is Na 2 SiO 3 .
[0018] Furthermore, the welding rod is pressed on a spiral coating machine.
[0019] Furthermore, the mass ratio of the coating outer skin to the welding core is 0.4:1 to 0.5:1.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1) Through the reasonable design of the welding core composition and the coating outer skin composition, the arc welding rod has high strength and high toughness; the yield strength of the cladding metal reaches more than 1000MPa, the tensile strength reaches more than 1100MPa, and the impact energy at -40℃ is not less than 47J.
[0022] 2) The arc welding rod of the present invention can be produced by conventional manufacturing methods without changing existing production equipment and processes.
[0023] 3) By using the arc welding rod of the present invention to weld 1000MPa high-strength steel, equal strength matching can be achieved, and the steel has the characteristics of high strength and good toughness.
[0024] 4) When the arc welding rod of the present invention is used, the weld seam will not crack at room temperature and welding without preheating can be achieved.
[0025] 5) The arc welding rod of the present invention is used to weld 1000MPa high-strength steel, which is simple, convenient and highly operable. DETAILED DESCRIPTION
[0026] The present invention discloses an arc welding rod for 1000MPa high-strength steel preheat-free welding, wherein the arc welding rod comprises a welding core and a coating outer skin coated on the outer side of the welding core; wherein the composition of the welding core is calculated by mass percentage as follows: C: 0.04%-0.08%, Si: 0.15%-0.35%, Mn: 1.85%-2.1%, Cr: 0.4%-0.6%, Ni: 4.5%-5.5%, Mo: 0.6%-0.9%, S≤0.008%, P≤0.010%, and the balance is iron; the composition of the coating outer skin is calculated by mass percentage as follows: CaCO 3 :24%~30%,SiO 2 :16%~21%,CaF 2 :18%~25%,TiO 2 : 10% ~ 15%, nano-TiN powder: 4% ~ 6.5%, and the rest is iron powder.
[0027] Furthermore, the average particle size of the nano-TiN powder is 20-45 nm.
[0028] The method for preparing an arc welding rod for preheat-free welding of 1000MPa high-strength steel of the present invention comprises the following steps:
[0029] (1) Drawing the welding wire steel wire rod into a welding wire with a diameter of 3.2 to 4.0 mm;
[0030] (2) Using a welding wire of a set length as a welding core; adding a coating used as a coating outer skin to an adhesive and mixing them evenly; in terms of mass percentage, the amount of the adhesive added is 15% to 20% of the total amount of the coating;
[0031] (3) Pressing the welding core and the coating mixed with the adhesive into a welding rod;
[0032] (4) Dry the welding rod at 360-400℃ for more than 2h to obtain arc welding rod.
[0033] Furthermore, the length of the welding wire as the welding core is 350 to 400 mm.
[0034] Further, the adhesive is Na 2 SiO 3 .
[0035] Furthermore, the welding rod is pressed on a spiral coating machine.
[0036] Furthermore, the mass ratio of the coating outer skin to the welding core is 0.4:1 to 0.5:1.
[0037] The reasons for designing the core composition in the arc welding rod of the present invention are as follows:
[0038] C: As the main strengthening element of the weld structure, it can improve the hardenability of the weld metal and the tensile strength of the weld. However, too high a carbon content will promote the formation of high-carbon martensite and increase the cold crack sensitivity of the weld metal. Therefore, the present invention controls the C content in the welding wire to 0.04% to 0.08%, while ensuring strength and reducing crack sensitivity to the greatest extent.
[0039] Si: Si element can play the role of solid solution strengthening and deoxidation in the weld. When Mn-Si exist at the same time, the deoxidation product can float up, so that the weld metal can be purified. In the present invention, since the coating coating also contains Si components, the Si content in the welding core is controlled to be 0.15% to 0.35%.
[0040] Mn: As the Mn content increases, the yield strength and tensile strength of the weld metal can be greatly improved, so Mn is a very effective weld strengthening element. However, when the Mn content is too high, the impact toughness of the weld metal will be greatly reduced, so the present invention controls the Mn element in the welding wire to be between 1.85% and 2.1%.
[0041] Cr: Cr is one of the important strengthening elements, which is beneficial to increase the content of acicular ferrite and reduce proeutectoid ferrite. However, when the Cr content is too high, brittle carbides are easily formed, which reduces the plasticity and toughness of the weld. Therefore, the present invention controls the Cr content to 0.4% to 0.6%.
[0042] Ni: Ni can reduce the ductile-brittle transition temperature, improve hardenability, and significantly improve the low-temperature impact toughness of the weld metal. However, Ni is a precious metal element and will increase the manufacturing cost of the welding rod. Therefore, the present invention controls the addition amount of Ni to 4.5% to 5.5%.
[0043] Mo: Mo can strongly delay the transformation of austenite and promote the formation of bainite and martensite in the weld metal, and is an important element for improving strength. By adjusting the amount of Mo and Mn added, the ratio of bainite, martensite and ferrite in the weld metal structure can be adjusted, so as to obtain a complex phase structure with good toughness, and at the same time, the stability of carbides can be improved, thereby improving the strength of the weld metal. The present invention controls the content of Mo to be between 0.6% and 0.9%.
[0044] The addition of nano TiN powder to the coating outer skin is an important feature of the present invention. 10% to 20% of the TiN powder added to the coating outer skin will directly transition to the molten pool. These TiN powders can play a beneficial role in pinning grain boundaries and hindering the growth of austenite grains, effectively improving the toughness of the weld. On the other hand, TiN can act as a hydrogen trap to hinder the diffusion of hydrogen atoms in the weld, thereby reducing crack sensitivity. The TiN content that can achieve the above purpose is 4% to 6%. If the TiN content is further increased, the probability of the occurrence of pore defects will increase.
[0045] The particle size of TiN is closely related to the fine crystal and the effect of hydrogen trap. The smaller the TiN size, the better the fine crystal and the effect of hydrogen trap. The present invention uses nano-scale TiN powder, which is an important means to ensure the realization of welding without preheating.
[0046] The following embodiments are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.
[0047] [Example]
[0048] In this embodiment, within the range of the welding core composition of the present invention, 4 furnaces of wire rods were smelted for wire drawing, and finally the obtained The welding core of Examples 1-4 is shown in Table 1. In this embodiment, a mixture for making the coating outer skin is configured within the composition range of the coating outer skin of the present invention. The coating outer skin compositions of Examples 1-4 are shown in Table 2.
[0049] This embodiment adopts the method for preparing arc welding rods of the present invention to manufacture welding rods, and the preparation process parameters of the welding rods are shown in Table 3.
[0050] In this embodiment, the pressed welding rods were used to carry out the cladding metal mechanical property test and the diffusible hydrogen test. The test results of Embodiments 1-4 are shown in Table 4.
[0051] In this embodiment, 1000MPa high-strength steel was welded using pressed welding rods, and 28mm steel plates were processed into V-shaped grooves. The welding current was 180A, the voltage was 25V, and the welding speed was 140mm / min. The tensile, impact and crack test results of the welded joints of Examples 1-4 are shown in Table 5.
[0052] Commercial high-strength steel arc welding rods were selected as comparative examples 1-3, and the same cladding metal experiments and welding joint experiments as in the embodiments were carried out. The results of each comparative example are also listed in Table 4, Table 5 and Table 6. Among them, comparative example 3 was not subjected to performance tests because of severe cracks.
[0053] Table 1 Welding core composition (Wt%)
[0054] C Si Mn P S Cr Ni Mo Fe Example 1 0.056 0.30 1.93 0.006 0.004 0.55 4.64 0.77 margin Example 2 0.072 0.17 1.95 0.007 0.003 0.52 5.38 0.81 margin Example 3 0.049 0.26 2.08 0.010 0.006 0.47 4.92 0.63 margin Example 4 0.061 0.24 1.90 0.008 0.005 0.43 4.78 0.80 margin
[0055] Table 2 Coating skin composition (Wt%)
[0056] <![CDATA[CaCO 3 ]]> <![CDATA[SiO 2 ]]> <![CDATA[CaF 2 ]]> <![CDATA[TiO 2 ]]> Nano TiN (average particle size) Iron Fan Example 1 26 18 20 12 4.5(32nm) margin Example 2 28 16.5 22 14.5 6(24nm) margin Example 3 25 17.5 24 11.5 5.5(41nm) margin Example 4 24 19 23.5 13 6.5(28nm) margin
[0057] Table 3 Welding rod preparation process parameters
[0058] Wire diameter, mm Adhesive, % Drying temperature, °C Drying time, h Example 1 3.8 18.5 375 2 Example 2 3.6 18 380 2.2 Example 3 3.2 17.5 395 2.5 Example 4 4.0 18 365 2.3
[0059] Table 4 Cladding metal properties
[0060]
[0061] Table 5 Welding conditions and crack notches
[0062] Preheating temperature Surface crack rate Section crack rate Root crack rate Example 1 15℃ 0 0 0 Example 2 15℃ 0 0 0 Example 3 15℃ 0 0 0 Example 4 15℃ 0 0 0 Comparative Example 1 150℃ 0 0 0 Comparative Example 2 100℃ 0 8% 15% Comparative Example 3 15℃ 11.5% 24.5% 63%
[0063] Table 6 Welding joint properties
[0064]
[0065] Note: Comparative Example 3 was not subjected to performance testing because of severe cracks.
[0066] It can be concluded from the above-mentioned Examples 1-4 and Comparative Examples 1-3 that the arc welding rod of the present invention overcomes the disadvantage of low strength of traditional welding rods and is suitable for 1000MPa steel welding. At the same time, the diffusible hydrogen content in the cladding metal is lower, the crack resistance is stronger, and welding without preheating can be achieved.
[0067] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. An arc welding rod for 1000MPa high-strength steel preheat-free welding, It is characterized in that The arc welding rod is composed of a welding core and a coating outer skin coated on the outside of the welding core; wherein the composition of the welding core is calculated by mass percentage as follows: C: 0.04%-0.08%, Si: 0.15%-0.35%, Mn: 1.85%-2.1%, Cr: 0.4%-0.6%, Ni: 4.5%-5.5%, Mo: 0.6%-0.9%, S≤0.008%, P≤0.010%, and the balance is iron; the composition of the coating outer skin is calculated by mass percentage as follows: CaCO 3 :24%~30%,SiO 2 :16%~21%,CaF 2 :18%~25%,TiO 2 : 10% ~ 15%, nano-TiN powder: 4% ~ 6.5%, and the rest is iron powder.
2. The arc welding rod for 1000MPa high-strength steel preheat-free welding according to claim 1, It is characterized in that The average particle size of the nano TiN powder is 20-45 nm.
3. A method for preparing an arc welding rod for 1000MPa high-strength steel preheat-free welding as claimed in claim 1 or 2, It is characterized in that The steps include: (1) Drawing the welding wire steel wire rod into a welding wire with a diameter of 3.2 to 4.0 mm; (2) Using a welding wire of a set length as a welding core; adding a coating used as a coating outer skin to an adhesive and mixing them evenly; in terms of mass percentage, the amount of the adhesive added is 15% to 20% of the total amount of the coating; (3) Pressing the welding core and the coating mixed with the adhesive into a welding rod; (4) Dry the welding rod at 360-400℃ for more than 2h to obtain arc welding rod.
4. A method for preparing an arc welding rod for 1000MPa high-strength steel preheat-free welding according to claim 3, It is characterized in that The length of the welding wire used as the welding core is 350 to 400 mm.
5. A method for preparing an arc welding rod for 1000MPa high-strength steel preheat-free welding according to claim 3, It is characterized in that The adhesive is Na 2 SiO 3 .
6. A method for preparing an arc welding rod for 1000MPa high-strength steel preheat-free welding according to claim 3, It is characterized in that The welding rod is pressed on a spiral press.
7. A method for preparing an arc welding rod for 1000MPa high-strength steel preheat-free welding according to claim 3, It is characterized in that The mass ratio of the coating outer skin to the welding core is 0.4:1 to 0.5:1.
Citation Information
Cited By
A welding rod and welding method for 1000mpa high-strength steel used in large-scale hydropower projects
CN122787649A