A styrene composition and preparation method thereof
By combining high-flow ethylene-butyl acrylate copolymer with high impact polystyrene resin and controlling impurity content, forming a 'skin-core' structure, the corrosion resistance and odor resistance of HIPS resin in harsh environments is solved, and the corrosion resistance and odor resistance of HIPS resin is achieved. The long-term stability and high performance of the material.
Patent Information
- Application Number
- CN202310406060.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-04-17
AI Technical Summary
High impact polystyrene (HIPS) resins have poor corrosion resistance when facing factors such as light, heat, oxygen, and water vapor, and there are odor problems caused by the residue of styrene monomers. The existing adsorbents cannot solve these problems for a long time. .
High-flow ethylene-butyl acrylate copolymer (EBA) and high impact polystyrene resin are used to form a 'skin-core' composite structure, and the impurity content in the composition is strictly controlled, and the twin-screw extruder is used to combine it with The dual vacuum extraction system removes impurities and reduces odor and erosion.
It significantly improves the weather resistance, heat and humidity resistance of the material, reduces odor properties, ensures stable use in harsh environments, and avoids discoloration and odor exceeding the standard.
Smart Images

Figure BDA0004181423370000071 
Figure BDA0004181423370000081 
Figure BDA0004181423370000082
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer alloy materials, and in particular to a styrene composition and a preparation method thereof. Background Art
[0002] High-impact polystyrene (HIPS) resin is an amorphous copolymer formed by the grafting reaction of styrene monomer and polybutadiene rubber. Its outstanding characteristics are easy processing, excellent dimensional stability, high impact strength and high rigidity. It can be processed by injection molding, extrusion, thermoforming, rotational molding, blow molding, foam molding, etc., and is widely used in household appliances, electronic appliances, building materials and tools, automobile transportation, toys and other product fields.
[0003] However, due to the presence of butadiene double bonds in HIPS resin, its corrosion resistance to factors such as light, heat, oxygen, and water vapor is relatively poor. When used in some light-colored or colored appearance parts, it is easily affected by external factors and undergoes obvious color changes. At the same time, due to the limitations of the synthesis process, the HIPS resin contains a large amount of residual styrene monomer, and styrene monomer has a pungent odor, which can be detected by the human sense of smell when the content in the air is 200-400ppm.
[0004] In response to the above problems, the prior art usually introduces adsorbents, especially odor adsorbents, such as molecular sieves, porous zeolites or diatomaceous earth, into the products. However, these adsorbents all have a certain adsorption saturation value without exception, and cannot effectively suppress the corrosion and odor problems of the products. They are also prone to negatively affect the physical properties of the products. In addition, the adsorption process of this type of adsorbent is a two-way diffusion process. During the subsequent use of the product, the adsorbed small molecules will be released again, resulting in excessive odor and decreased corrosion resistance. On the other hand, in addition to the use of adsorbents, there are also methods of adding jellyfish particles or liquid injection processes to improve the performance of the product using the devolatilization effect, but this method does not significantly improve the odor. Summary of the invention
[0005] Based on the defects of the prior art, the purpose of the present invention is to provide a styrene composition, which is mainly composed of high-impact polystyrene resin and high-fluidity ethylene-butyl acrylate copolymer (EBA) as a component, and at the same time limits the impurity content of the composition to a relatively low range. The composition not only has excellent corrosion resistance in terms of weather resistance, heat resistance, moisture resistance and other factors, but also does not have a discoloration effect; at the same time, it has low odor and stable properties, and can be used in various harsh environments.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A styrene composition comprising the following components in parts by weight:
[0008] 70-85 parts of high impact polystyrene resin, 5-10 parts of ethylene-butyl acrylate copolymer, 2-5 parts of compatibilizer, 2-5 parts of toughening agent, 0.5-1 part of weathering agent;
[0009] The high-impact polystyrene resin has a melt flow rate of 3 to 8 g / 10 min at 200° C. and a load of 5 kg according to ISO 1133-1-2011, and the ethylene-butyl acrylate copolymer has a melt flow rate of 20 to 100 g / 10 min at 190° C. and a load of 2.16 kg according to ISO 1133-1-2011;
[0010] The TVOC content of the styrene composition is ≤0.03 wt %.
[0011] The styrene composition of the present invention contains impurities including residual monomers such as styrene, ethylbenzene and / or toluene and other impurities, so the total volatile organic matter TVOC is used for calculation.
[0012] Preferably, the TVOC is measured according to TS-INT-002-2008, and the test method is as follows: firstly, the sample is broken into small pieces of 10-25 mg, then 1.200±0.0001 g of the sample is weighed and put into a headspace bottle, the bottle is sealed and heated at 120°C for 5 hours, and three headspace bottles are made in parallel for each sample. A syringe is inserted into the bottle to transmit the volatile organic matter to a gas chromatograph (GC) for testing.
[0013] In the prior art, people often use adsorbents to absorb impurity molecules originally present in styrene products or produced by external factors to reduce their odor and erosion, but the effect of this method is not thorough and long-lasting. In the styrene composition of the present invention, ethylene-butyl acrylate copolymer is introduced into high-impact polystyrene resin as a modified component. Since ethylene-butyl acrylate copolymer has high fluidity, it will be enriched on the surface of the product when mixed with a high-impact polystyrene resin with low fluidity, forming a composite structure similar to "skin-core", effectively inhibiting external oxygen, water vapor and other substances from contacting the high-impact polystyrene resin, and reducing the discoloration probability of the high-impact polystyrene resin. If the fluidity of the introduced ethylene-butyl acrylate copolymer is too low, it cannot form a specific composite structure, and if the fluidity of the ethylene-butyl acrylate copolymer is too high, it will directly affect the toughness of the product, causing the impact resistance of the product to significantly decrease, and it cannot meet the use requirements. At the same time, ethylene-butyl acrylate copolymer has excellent thermal stability, heat sealing and water-proof properties, which significantly improves the overall corrosion resistance of the product. Ethylene-butyl acrylate copolymer has good impact resistance and can also be used as a toughening agent when combined with high-impact polystyrene resin. This component has high polarity and good compatibility with other components, so it can effectively reduce the amount of functional additives such as toughening agents and compatibilizers added to the product components, and avoid excessive by-products when these components are oxidized and deteriorated during product processing and use. At the same time, the inventors also strictly control the TVOC content in the styrene composition, significantly reducing the odor and the possibility of erosion, ensuring the long-term stability of the product.
[0014] Preferably, the high-impact polystyrene resin is at least one of new high-impact polystyrene resin and recycled high-impact polystyrene resin.
[0015] More preferably, the melt flow rate of the new high-impact polystyrene resin material at 200°C and 5kg load is 4-8g / 10min according to ISO1133-1-2011; the melt flow rate of the recycled high-impact polystyrene resin material at 200°C and 5kg load is 3-5g / 10min according to ISO1133-1-2011.
[0016] Generally speaking, compared with new materials, high-impact polystyrene resin recycled materials have more impurity molecules, worse corrosion resistance, and a higher probability of yellowing. However, in the styrene composition described in the present invention, due to the introduction of ethylene-butyl acrylate copolymer and strict control of product impurities, even if high-impact polystyrene resin recycled materials are used as components, the performance and stability of the final product can still be guaranteed, while significantly improving the environmental friendliness of the product.
[0017] Preferably, the ethylene-butyl acrylate copolymer has a melt flow rate of 30 to 60 g / 10 min at 190° C. and a load of 2.16 kg according to ISO 1133-1-2011.
[0018] Since the fluidity of the ethylene-butyl acrylate copolymer itself is related to the stability of the product's composite structure and the compatibility of each component, as the fluidity increases, the product's impact resistance decreases. At the same time, the dispersibility of components such as the weathering agent it carries will also decrease to a certain extent. Therefore, the use of ethylene-butyl acrylate copolymer within the above range has the best effect.
[0019] Preferably, the compatibilizer is at least one of styrene-ethylene-butylene-styrene block copolymer and styrene-ethylene / propylene-styrene block copolymer.
[0020] Preferably, the toughening agent is at least one of styrene-butadiene-styrene block copolymer and styrene-isoprene-styrene block copolymer.
[0021] Preferably, the weathering agent is at least one of a light stabilizer and an ultraviolet light absorber.
[0022] More preferably, the weathering agent is a mixture of a light stabilizer and an ultraviolet light absorber, and the mass ratio of the two is (0.8-1.2): (0.8-1.2).
[0023] More preferably, the light stabilizer is a hindered amine light stabilizer, and the ultraviolet light absorber is a benzotriazole ultraviolet light absorber.
[0024] Through the specific combination of weathering agents, the light resistance of the styrene composition can be effectively improved. At the same time, each compound has stable properties and good compatibility with ethylene-butyl acrylate copolymer, and it is enriched on the product surface together with it to form an effective high-impact polystyrene resin "protective film".
[0025] Preferably, the components of the styrene composition also include 0 to 2 parts by weight of a processing aid, wherein the processing aid is a mixture of an antioxidant and a lubricant, wherein the antioxidant is at least one of a hindered phenol antioxidant and a phosphite antioxidant; and the lubricant is at least one of vinyl bisstearamide, polysiloxane, calcium stearate, magnesium stearate, zinc stearate, PE wax, and PP wax.
[0026] Another object of the present invention is to provide a method for preparing the styrene composition, comprising the following steps:
[0027] After the components are uniformly mixed, they are fed into a twin-screw extruder from a main feeding port for melt blending and extrusion. At the same time, water is added to the screw barrels of the first and second zones of the twin-screw extruder, and a foaming agent is added to the side feeding port of the twin-screw extruder. During the melt blending and extrusion process, a double vacuum extraction system is used for extraction treatment. The obtained material body is water-cooled, pelletized, and dried to obtain the styrene composition.
[0028] In the preparation method of the styrene composition of the present invention, in order to limit the impurity content of the obtained product, water is added in the front section of the component melt blending extrusion process, and a foaming agent is added in the middle section. The water vapor and gas generated by the water and the foaming agent when heated are used to activate the impurities and monomers in the components, and then these impurities and monomers are extracted by a double vacuum extraction system to improve the purity of the product. At the same time, there is no need to introduce adsorbents, which are not only poor in efficacy but also may affect the physical properties of the product. Since the water and the foaming agent are extracted and separated by entraining impurities and monomers after being heated, they will not remain in the product and will not affect the purity and physical properties of the product. The preparation method has simple operation steps and can be mass-produced.
[0029] Preferably, the mass ratio of high impact polystyrene resin, water and blowing agent in the components of the styrene composition is high impact polystyrene resin: water: blowing agent = (70-85): (1-5): (2-8).
[0030] Since water and foaming agent are respectively added in the front section and middle section of the component blending and melt extrusion, their added content is related to the degree of activation and entrainment of impurities and monomers in the components. They need to be maintained within a specific range to extract impurities and monomers to the maximum extent without excessively affecting the physical properties of the original components. Water or foaming agent alone cannot achieve the expected extraction effect.
[0031] Preferably, the foaming agent is a foaming agent masterbatch, and more preferably, the foaming agent masterbatch is a carbonate foaming agent loaded polystyrene resin masterbatch, and the loading amount of the carbonate foaming agent is 30-50wt%.
[0032] Introducing the foaming agent in the form of a masterbatch, especially using a polystyrene resin of the same type as the base resin in the component as a masterbatch carrier, can achieve a better dispersion of the foaming agent in the component and a better effect of entraining and extracting impurities and monomers.
[0033] Preferably, when the components are melt-blended and extruded, the temperature of zones 1 to 2 of the twin-screw extruder is 120°C to 190°C, the temperature of zones 3 to 5 is 200°C to 240°C, the temperature of zones 5 to 12 is 200°C to 240°C, the aspect ratio of the screw is (48 to 60): 1, and the rotation speed is 350rpm to 450rpm; the dual vacuum extraction system is two vacuum extraction systems arranged in zones 5 to 7 and zones 9 to 11, and the vacuum degree is controlled at 0.05 to 0.09Mpa.
[0034] Another object of the present invention is to provide the use of the styrene composition in the preparation of electrical appliances, office supplies, building materials, and vehicle parts. Preferably, the styrene composition is used in automotive interior trims.
[0035] The styrene composition of the present invention has good impact resistance due to the selection of the base resin itself, and also has excellent corrosion resistance and yellowing resistance, and has high stability in various external use environments. At the same time, compared with other styrene products, the product has less odor, and is therefore very suitable for the preparation of products in multiple fields with harsh and diverse use environments and high requirements for odor and appearance.
[0036] The beneficial effect of the present invention is that the present invention provides a styrene composition, which is mainly composed of high-impact polystyrene resin and high-fluidity ethylene-butyl acrylate copolymer as a component, and at the same time limits the impurity content of the composition to a relatively low range. It not only has excellent corrosion resistance of multiple factors such as weather resistance, heat resistance, and moisture resistance, but also does not cause discoloration effect; at the same time, it has low odor and stable properties, and can be used in various harsh environments. DETAILED DESCRIPTION
[0037] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work premise belong to the protection scope of the present invention. The experimental reagents and instruments involved in the implementation of the present invention, unless otherwise specified, are all commonly used common reagents and instruments.
[0038] Examples 1 to 12
[0039] The embodiments of the styrene composition and the preparation method thereof of the present invention, the components of the styrene composition and the processing raw material components are shown in Table 1.
[0040] The preparation method of the styrene composition comprises the following steps:
[0041] After the components are uniformly mixed, they are fed into a twin-screw extruder from a main feeding port for melt blending and extrusion. At the same time, water is added at the screw barrel of the first and second zones of the twin-screw extruder using a liquid pump, and a foaming agent is added at the side feeding port of the twin-screw extruder. During the melt blending and extrusion process, a double vacuum extraction system is used for extraction treatment. The obtained material body is water-cooled, pelletized, and dried to obtain the styrene composition.
[0042] When the components are melt-blended and extruded, the temperature of the first to second zones of the twin-screw extruder is 120°C to 190°C, the temperature of the third to fifth zones is 200°C to 240°C, the temperature of the fifth to twelfth zones is 200°C to 240°C, the aspect ratio of the screw is (48 to 60): 1, and the rotation speed is 350rpm to 450rpm; the dual vacuum extraction system refers to installing vacuum extraction systems in the fifth to seventh zones and the ninth to eleventh zones respectively, and the vacuum degree is controlled at 0.05 to 0.09Mpa.
[0043] Comparative Examples 1 to 10
[0044] The difference between the comparative examples and the embodiments is only in the types and proportions of components, as shown in Table 2.
[0045] It should be noted that in Tables 1 and 2, when the added weight of water or foaming agent is 0, it means that no water or foaming agent is added in the twin-screw extruder during the product preparation process, and when the other components are 0, it indicates that the styrene composition does not contain the substance.
[0046] Among the components described in each embodiment and comparative example,
[0047] The high-impact polystyrene resin 1 is PS MA5210 produced by Yased Chemical, a new material, with a melt flow rate of 5 g / 10 min at 200° C. and a load of 5 kg, and a TVOC content of 0.06 wt %;
[0048] The high-impact polystyrene resin 2 is LRHPS-BCWA1134 (KS) produced by Guangdong Kingfa Technology, a recycled material, with a melt flow rate of 4 g / 10 min at 200° C. and a load of 5 kg, and a TVOC content of 0.12 wt%;
[0049] The high-impact polystyrene resin 3 is HIPS N6502 produced by LyondellBasell, a new material, with a melt flow rate of 21 g / 10 min at 200° C. and a load of 5 kg, and a TVOC content of 0.07 wt %;
[0050] The ethylene-butyl acrylate copolymer 1 is EBA AC34035 produced by Dow Chemical of the United States, and has a melt flow rate of 40 g / 10 min at 190° C. and a load of 2.16 kg;
[0051] The ethylene-butyl acrylate copolymer 2 is EBA 35BA40 produced by Arkema, France, and has a melt flow rate of 50 g / 10 min at 190° C. and a load of 2.16 kg;
[0052] The ethylene-butyl acrylate copolymer 3 is EBA E20020 produced by Repsol, Spain, and has a melt flow rate of 20 g / 10 min at 190° C. and a load of 2.16 kg;
[0053] The ethylene-butyl acrylate copolymer 4 is EBA 28BA100 produced by Arkema, France, and has a melt flow rate of 100 g / 10 min at 190° C. and a load of 2.16 kg;
[0054] The ethylene-butyl acrylate copolymer 5 is EBA 1400HN produced by Lucobi, Germany, and has a melt flow rate of 1.4 g / 10 min at 190° C. and a load of 2.16 kg;
[0055] The ethylene-butyl acrylate copolymer 6 is EBA E27150 produced by Repsol of Spain, and has a melt flow rate of 150 g / 10 min at 190° C. and a load of 2.16 kg;
[0056] The ethylene-vinyl acetate copolymer is EVA 240W produced by Dow Chemical of the United States, and has a melt flow rate of 43 g / 10 min at 190° C. and a load of 2.16 kg;
[0057] Compatibilizer: SEBS 7551 produced by Li Changrong Chemical, styrene-ethylene-butylene-styrene block copolymer;
[0058] Toughener: GLOBALPRENE 3566 produced by Li Changrong Chemical, styrene-butadiene-styrene block copolymer;
[0059] Weathering agent: a mixture of commercially available hindered amine light stabilizer and benzotriazole ultraviolet light absorber in a mass ratio of 1:1;
[0060] Antioxidant: a mixture of commercially available hindered phenol antioxidant and phosphite antioxidant in a mass ratio of 1:1;
[0061] Lubricant: Commercially available vinyl bisstearamide;
[0062] Foaming agent: F-53 produced by Yonghe Fine Chemicals, foaming agent masterbatch, the foaming agent is sodium bicarbonate, the foaming agent content is 40±2wt%, and the base resin is styrene resin;
[0063] Adsorbent: Diatomaceous earth K837167 produced by Shanghai McLean Biochemical Technology Co., Ltd.
[0064] Unless otherwise specified, the components and raw materials used in the embodiments and comparative examples of the present invention are all commercially available raw materials, and the components and raw materials used in each parallel experiment are all of the same kind.
[0065] Each example and comparative example product needs to be broken into small pieces of 10-25 mg, and then 1.200±0.0001 g of the sample is weighed and placed in a headspace bottle, the bottle is sealed and heated at 120°C for 5 hours, and three headspace bottles are made in parallel for each sample. A syringe is inserted into the bottle to transmit the volatile organic matter to a gas chromatograph (GC) for testing, and the TVOC content is finally determined.
[0066] Table 1
[0067]
[0068]
[0069] Table 2
[0070]
[0071] In order to verify the performance of the styrene composition of the present invention, the products prepared in each embodiment and comparative example were subjected to the following performance tests, and the specific steps are as follows:
[0072] (1) Notched impact strength test: According to ISO 180-2019 standard, each product was injection molded into an impact specimen with a size of 80×10×4 mm and tested using an A-notch;
[0073] (2) Odor level test: According to the PV3900E standard of Volkswagen, Germany, the evaluation is graded from 1 to 6. The higher the grade, the stronger the odor. The test method is: take 200g ± 10g of the product and place it in a sealed glass container, bake it in an oven at 80 ± 2℃ for 2h, cool it to 60 ± 5℃, and place it at room temperature for 5min. At least three professionals will give the odor score based on their sense of smell and calculate the average value.
[0074] (3) Heat and humidity light aging performance: The product was tested in accordance with ASTM D4459-2012 standard, and was continuously exposed to a xenon lamp for 72 hours, and then aged in a constant temperature and humidity chamber at 85°C / 85%RH for 72 hours. The color difference △E of the product before and after was measured using a CWF light source in accordance with GB / T 7921-2008 standard. The larger the color difference, the worse the product's resistance to heat and humidity light aging performance.
[0075] The test results are shown in Tables 3 and 4.
[0076] Table 3
[0077]
[0078]
[0079] Table 4
[0080]
[0081] As can be seen from Tables 3 and 4, the styrene composition of the present invention has a "skin-core" structure formed by combining high-impact polystyrene resin and ethylene-butyl acrylate copolymer in the components, and effectively controls the impurity components in the product. Therefore, it not only has good notched impact strength (≥10KJ / m2), but also has a significantly lower odor level than existing products to 3.5 and below, and the color difference △E can also be maintained at 2, with a minimum of 0.5 or below, and has excellent corrosion resistance and stability. According to the products of Examples 1 to 3, it can be clearly seen that the product formula is effective for high-impact polystyrene resin, whether it is new material or recycled material, and ethylene-butyl acrylate copolymer has the effect of synergistically toughening high-impact polystyrene and improving stability. In contrast, the product of Comparative Example 1 does not introduce ethylene-butyl acrylate copolymer, nor does it remove impurities. The impurity content of the product components is high, which not only fails to achieve good notched impact strength, but also has a large odor and insufficient stability; although the product of Comparative Example 2 introduces ethylene-butyl acrylate copolymer, it still does not control the impurity content, and the odor level and color difference of the product do not meet expectations. In the product of Comparative Example 9, impurities are controlled, but ethylene-butyl acrylate copolymer is not introduced. It can be seen that the notched impact strength and color difference of the product are not as good as those of the embodiment product, indicating that ethylene-butyl acrylate copolymer has an improvement effect on both properties. The fluidity of the ethylene-butyl acrylate copolymer introduced in Comparative Examples 3 and 4 is too low or too high, and the product cannot take into account both the notched impact strength and discoloration. In the product of Comparative Example 5, ethylene-vinyl acetate copolymer is used instead of ethylene-butyl acrylate copolymer. It can be seen that its compatibility with high-impact polystyrene resin is not ideal. The prepared styrene composition not only has low notched impact strength, but also has a large odor, and the grade reaches level 4. In the product of Comparative Example 6, a high-impact polystyrene resin with too high fluidity is used as a component. Its own molecular weight is low and its toughness is extremely low. Therefore, even if ethylene-butyl acrylate copolymer is introduced, it is difficult to achieve the ideal notched impact strength. At the same time, it and ethylene-butyl acrylate copolymer cannot form a "skin-core" structure, so naturally it cannot achieve a good corrosion resistance effect, and the long-term stability is poor. In the process of controlling impurities, water and foaming agent were not introduced simultaneously during the preparation of the products of Comparative Examples 7 and 8, so the impurity content thereof could not be controlled below 0.03 wt %, and the product performance was poor.
[0082] It can be seen from Comparative Example 10 that although the introduction of an additional adsorbent, diatomaceous earth, into the existing product can indeed improve the impurity and odor situation to a certain extent, the effect is not obvious and the impurity content of the product cannot be reduced to ≤0.03wt%.
[0083] Embodiment 13
[0084] Further, in order to verify the universality of the styrene composition of the present invention for the preparation method, this example is prepared according to the following process, which is the same as Example 1 except for the following:
[0085] After the components are mixed evenly, they are fed into a twin-screw extruder from the main feed port for melt blending and extrusion. During the melt blending and extrusion process, a double vacuum extraction system is used for extraction treatment; the obtained material is water-cooled, pelletized, and dried to obtain the styrene composition. The high-impact polystyrene resin 1 is replaced by high-impact polystyrene 4, HIPS HIE-1 produced by Dushanzi Petrochemical, a new material, with a melt flow rate of 3.5g / 10min at 200°C and a load of 5kg, and a TVOC content of 0.031wt%.
[0086] The product prepared in Example 13 was analyzed and tested, and the test results are as follows:
[0087] The TVOC content of the product is 0.03wt%, and the notched impact strength is 12.5KJ / m 2 , the odor level is 3.5, and the color difference △E is 1.63.
[0088] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A styrene composition, characterized in that The composition comprises the following components in parts by weight: 70-85 parts of high impact polystyrene resin, 5-10 parts of ethylene-butyl acrylate copolymer, 2-5 parts of compatibilizer, 2-5 parts of toughening agent, 0.5-1 part of weathering agent; The melt flow rate of the high impact polystyrene resin at 200° C. and 5 kg load is 3-8 g / 10 min, and the melt flow rate of the ethylene-butyl acrylate copolymer at 190° C. and 2.16 kg load is 20-100 g / 10 min; Water and a foaming agent are added when the components of the styrene composition are melt-blended and extruded, and the TVOC content of the styrene composition is ≤0.03wt%.
2. The styrene composition according to claim 1, characterized in that: The high-impact polystyrene resin is at least one of new high-impact polystyrene resin and recycled high-impact polystyrene resin.
3. The styrene composition according to claim 2, characterized in that: The melt flow rate of the new high-impact polystyrene resin material at 200° C. and a load of 5 kg is 4-8 g / 10 min; the melt flow rate of the recycled high-impact polystyrene resin material at 200° C. and a load of 5 kg is 3-5 g / 10 min.
4. The styrene composition according to claim 1, characterized in that: The melt flow rate of the ethylene-butyl acrylate copolymer at 190° C. and a load of 2.16 kg is 30-60 g / 10 min.
5. The styrene composition according to claim 1, characterized in that: The compatibilizer is at least one of styrene-ethylene-butylene-styrene block copolymer and styrene-ethylene / propylene-styrene block copolymer; the toughening agent is at least one of styrene-butadiene-styrene block copolymer and styrene-isoprene-styrene block copolymer; the weathering agent is at least one of a light stabilizer and an ultraviolet light absorber.
6. The styrene composition according to claim 5, characterized in that The light stabilizer is a hindered amine light stabilizer, and the ultraviolet light absorber is a benzotriazole ultraviolet light absorber.
7. The styrene composition as claimed in claim 1, characterized in that, The components of the styrene composition also include 0 to 2 parts by weight of a processing aid, which is a mixture of an antioxidant and a lubricant, wherein the antioxidant is at least one of a hindered phenol antioxidant and a phosphite antioxidant; and the lubricant is at least one of vinyl bisstearamide, polysiloxane, calcium stearate, magnesium stearate, zinc stearate, PE wax, and PP wax.
8. The method for preparing a styrene composition according to any one of claims 1 to 7, characterized in that: The following steps are involved: After the components are uniformly mixed, they are fed into a twin-screw extruder from a main feeding port for melt blending and extrusion. At the same time, water is added to the screw barrels of the first and second zones of the twin-screw extruder, and a foaming agent is added to the side feeding port of the twin-screw extruder. During the melt blending and extrusion process, a double vacuum extraction system is used for extraction treatment. The obtained material body is water-cooled, pelletized, and dried to obtain the styrene composition.
9. The method for preparing a styrene composition according to claim 8, characterized in that: The mass ratio of high-impact polystyrene resin, water and foaming agent in the components of the styrene composition is high-impact polystyrene resin: water: foaming agent = (70-85): (1-5): (2-8); the foaming agent is a foaming agent masterbatch.
10. The method for preparing a styrene composition according to claim 9, characterized in that: The foaming agent masterbatch is a carbonate foaming agent loaded polystyrene resin masterbatch.
11. The method for preparing a styrene composition according to claim 8, wherein: When the components are melt-blended and extruded, the temperature of zones 1 to 2 of the twin-screw extruder is 120°C to 190°C, the temperature of zones 3 to 5 is 200°C to 240°C, the temperature of zones 5 to 12 is 200°C to 240°C, the aspect ratio of the screw is (48 to 60): 1, and the rotation speed is 350 rpm to 450 rpm; the dual vacuum extraction system is two vacuum extraction systems arranged in zones 5 to 7 and zones 9 to 11, and the vacuum degree is controlled at 0.05 to 0.09 MPa.
12. Use of the styrene composition according to any one of claims 1 to 7 or the styrene composition obtained by the preparation method according to any one of claims 8 to 11 in the preparation of electrical appliances, office supplies, building materials, and vehicle parts.