A kind of sulfuric acid-containing environmental antibacterial coating and preparation method thereof
By preparing microcapsule coatings containing organic antibacterial agents, the problem of unstable antibacterial performance in sulfuric environments under existing technologies has been solved, achieving long-lasting antibacterial and corrosion-resistant effects in the oil and gas industry.
Patent Information
- Application Number
- CN202210133712.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-14
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-02-14
AI Technical Summary
Existing technologies cannot guarantee stable antibacterial and bactericidal properties in sulfuric acid environments and cannot adapt to the harsh environments of the oil and gas industry.
Antibacterial microcapsules were prepared using organic antibacterial agents as the core material and dispersed in epoxy resin materials to form an antibacterial coating. Using epoxy resin and organic solvents as the main components, along with suitable shell materials and emulsifiers, an antibacterial coating adapted to sulfuric acid environments was prepared.
The prepared antibacterial coating exhibits good antibacterial properties and corrosion resistance in a sulfuric acid environment, making it suitable for pipelines and equipment in the oil and gas industry. It also has a long-lasting antibacterial effect and good weather resistance.
Smart Images

Figure BDA0003503690490000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to an antibacterial coating for a sulfuric acid-containing environment and a preparation method thereof. Background Art
[0002] In the process of oil and gas extraction, the extracted crude oil and natural gas often contain a large number of microorganisms, which cause serious corrosion to the transmission pipelines and equipment, affecting the service life. At the same time, the water produced by crude oil and natural gas usually contains a large amount of minerals, which are easy to scale in the pipelines or processing equipment, leading to the growth and reproduction of microorganisms, further aggravating the corrosion of the transmission pipelines and equipment in the oil and gas fields.
[0003] Although a variety of antibacterial and bactericidal coatings have been proposed in the prior art, there is no bactericidal and antibacterial coating specifically for the oil and gas development industry. The publicly available bactericidal and antibacterial coatings are also difficult to adapt to the harsh environment of the oil and gas industry, especially in a sulfuric acid environment, it is difficult to ensure stable antibacterial and bactericidal properties. Summary of the invention
[0004] In order to solve the problem that the prior art is difficult to ensure stable antibacterial and bactericidal performance in a sulfuric acid environment, the present invention provides an antibacterial coating for a sulfuric acid environment and a preparation method thereof.
[0005] The technical solution of the present invention is as follows:
[0006] A sulfuric acid-containing environmental antibacterial coating, characterized in that it comprises component A and component B, wherein component A comprises epoxy resin, organic solvent, emulsifier and antibacterial microcapsules; component B comprises organic solvent and curing agent; the antibacterial microcapsules use organic antibacterial agent as core material and use any one of maltodextrin, alginate, epoxy resin or polyacrylonitrile as shell material; the raw materials of component A are calculated by mass: 20-30 parts of epoxy resin, 25-40 parts of organic solvent, 2-10 parts of emulsifier, and 5-15 parts of antibacterial microcapsules; the raw materials of component B are calculated by mass: 30-50 parts of organic solvent and 25-40 parts of curing agent.
[0007] Preferably, the organic antibacterial agent is N-(trichloromethyl)-thiophthalimide and / or 2-bromo-2-nitropropane-1,3-diol.
[0008] Preferably, the embedding rate of the organic antibacterial agent in the microcapsule is not less than 10%.
[0009] Preferably, the component A further comprises a filler, a defoamer and a leveling agent, wherein the filler accounts for 10 to 15 parts by mass; the defoamer accounts for 0.5 to 3 parts by mass; and the leveling agent accounts for 1 to 3 parts by mass.
[0010] Preferably, the curing agent is one or more of phenolic resin, polyamide, and aliphatic polyamine.
[0011] Preferably, the emulsifier includes one or more of OP-10, sodium dodecyl sulfate, and multi-block copolymer PEG-(EP-PEG)3-EP-PEG.
[0012] The aforementioned method for preparing an antibacterial coating for a sulfuric acid environment is characterized by comprising the following steps:
[0013] S1) preparing antibacterial microcapsules;
[0014] S2) preparing component A and component B respectively;
[0015] S3) Add component B to component A, and stir and disperse them evenly to obtain the coating for use.
[0016] Preferably, step S1) comprises the following steps:
[0017] S11) preparing an emulsified system: adding the shell material to deionized water, heating to 50-70° C., stirring and mixing evenly, adding a shell material emulsifier, stirring and emulsifying, and obtaining a stable emulsified system;
[0018] S12) adding an organic antibacterial agent to the emulsified system, maintaining a constant temperature, and continuously stirring to coat the system to obtain antibacterial microcapsules, which are then dried and prepared into powder for later use.
[0019] More preferably, the shell material emulsifier is one or any two of octenyl succinate starch ester, sucrose ester, monoglyceride, carrageenan, modified starch, and gum arabic.
[0020] Preferably, step S2) comprises the following steps:
[0021] S21) Preparation component A:
[0022] S211) Preparation of antibacterial microcapsule dispersion: Add the antibacterial microcapsules prepared in step S1) into deionized water, stir and mix evenly to obtain an antibacterial microcapsule dispersion:
[0023] S212) adding epoxy resin to an organic solvent, stirring and dissolving, then adding an emulsifier, heating to 60-80° C., and continuing to stir to emulsify, to obtain a stable epoxy resin emulsified system; then adding an antibacterial microcapsule dispersion to the epoxy resin emulsified system, continuing to stir and mix evenly, to obtain component A;
[0024] S22) preparing component B: dissolving the curing agent in an organic solvent to obtain component B.
[0025] Further preferably, step S21) further includes S213): adding filler, defoamer and leveling agent to component A, stirring and mixing evenly to obtain component A to be used.
[0026] The technical effects of the present invention are as follows:
[0027] The invention discloses an antibacterial coating for a sulfuric acid environment, wherein an organic antibacterial agent is used as a core material to prepare a microcapsule containing the antibacterial agent, and the microcapsule is dispersed in a resin material to form an antibacterial coating with good antibacterial property, long-lasting antibacterial performance, good weather resistance and not easy to change color. Commonly used epoxy resins and organic solvents can be used.
[0028] Preferably, maltodextrin with good acid resistance is used as the shell material of the microcapsule, and N-(trichloromethyl)-thiophthalimide and / or 2-bromo-2-nitropropane-1,3-diol are used as organic antibacterial agents. They have good antibacterial effects, can adapt to the sulfuric acid environment of oil and gas fields, have long-lasting antibacterial properties, and have good corrosion resistance.
[0029] The invention discloses a method for preparing an antibacterial coating for an environment containing sulfuric acid. The method is simple, and the prepared antibacterial coating has long-lasting and good antibacterial performance and good corrosion resistance, and is suitable for an environment containing sulfuric acid. DETAILED DESCRIPTION
[0030] In order to better understand the present invention, the following is a further description in conjunction with specific embodiments. The present invention is not limited by the following embodiments, and the specific implementation method can be determined according to the technical solution of the present invention and actual conditions.
[0031] Example 1
[0032] A sulfuric acid-containing antibacterial paint, with the following formula: the raw materials of component A are calculated by mass: 20 parts of epoxy resin, 30 parts of organic solvent, 2 parts of emulsifier, 5 parts of antibacterial microcapsules, 15 parts of filler, 3 parts of defoamer, and 3 parts of leveling agent; the raw materials of component B are calculated by mass: 40 parts of organic solvent and 25 parts of curing agent.
[0033] The antibacterial coating is prepared by the following method:
[0034] S1) preparing antibacterial microcapsules;
[0035] S11) preparing an emulsified system: adding shell material maltodextrin to deionized water, heating to 50° C., stirring and mixing evenly, adding shell material emulsifier sucrose ester, stirring at a speed of 500 r / min for 15 min to emulsify, and obtaining a stable emulsified system;
[0036] S12) adding the organic antibacterial agent N-(trichloromethyl)-thiophthalimide to the emulsified system in a mass ratio of 1:5 between the organic antibacterial agent and the shell material maltodextrin, maintaining the temperature at 50° C., and continuing to stir for 20 min for coating to obtain antibacterial microcapsules, which are then dried and prepared into powder for later use.
[0037] S2) preparing component A and component B respectively;
[0038] S21) Preparation component A:
[0039] S211) Preparation of antibacterial microcapsule dispersion: Weigh antibacterial microcapsules according to the formula ratio, add the antibacterial microcapsules prepared in step S1) into deionized water at a mass ratio of 1:1, stir and mix evenly to obtain an antibacterial microcapsule dispersion:
[0040] S212) adding epoxy resin to organic solvent acetone according to the formula ratio, stirring, then adding emulsifier sodium dodecyl sulfate, heating to 60° C., and stirring for 20 min to emulsify it to obtain a stable epoxy resin emulsified system; then adding antibacterial microcapsule dispersion to the epoxy resin emulsified system, and stirring for 30 min to mix evenly;
[0041] S213): Add filler, defoamer and leveling agent to component A, stir and mix evenly to obtain component A to be used.
[0042] S22) preparing component B: adding a curing agent phenolic resin into an organic solvent acetone to obtain component B.
[0043] S3) Add component B to component A, and stir and disperse them evenly to obtain coating A for use.
[0044] Example 2
[0045] A sulfuric acid-containing antibacterial paint, with the following formula: the raw materials of component A are calculated by mass: 30 parts of epoxy resin, 40 parts of organic solvent, 10 parts of emulsifier, 15 parts of antibacterial microcapsules, 10 parts of filler, 0.5 parts of defoamer, and 1 part of leveling agent; the raw materials of component B are calculated by mass: 50 parts of organic solvent and 40 parts of curing agent.
[0046] The antibacterial coating is prepared by the following method:
[0047] S1) preparing antibacterial microcapsules;
[0048] S11) preparing an emulsified system: adding the shell material alginate to deionized water, heating the mixture to 70° C., stirring and mixing the mixture evenly, adding the shell material emulsifier carrageenan, stirring the mixture at a speed of 500 r / min for 10 min to emulsify the mixture, and obtaining a stable emulsified system;
[0049] S12) adding the organic antibacterial agent N-(trichloromethyl)-thiophthalimide to the emulsified system in a mass ratio of 1:8 between the organic antibacterial agent and the alginate, maintaining the temperature at 70° C., and continuing to stir for 10 min for coating to obtain antibacterial microcapsules, which are then dried and prepared into powder for later use.
[0050] S2) preparing component A and component B respectively;
[0051] S21) Preparation component A:
[0052] S211) Preparation of antibacterial microcapsule dispersion: Weigh antibacterial microcapsules according to the formula ratio, add the antibacterial microcapsules prepared in step S1) into deionized water at a mass ratio of 1:1, stir and mix evenly to obtain an antibacterial microcapsule dispersion:
[0053] S212) adding epoxy resin to organic solvent acetone according to the formula ratio, stirring, then adding emulsifier OP-10, heating to 80° C., and stirring for 10 min to emulsify it to obtain a stable epoxy resin emulsified system; then adding antibacterial microcapsule dispersion to the epoxy resin emulsified system, and stirring for 20 min to mix evenly;
[0054] S213): Add filler, defoamer and leveling agent to component A, stir and mix evenly to obtain component A to be used.
[0055] S22) preparing component B: dissolving the curing agent in an organic solvent to obtain component B.
[0056] S3) adding component B to component A, and stirring and dispersing the component A to obtain coating B for use.
[0057] Example 3
[0058] A sulfuric acid-containing antibacterial paint, with the following formula: the raw materials of component A are calculated by mass: 25 parts of epoxy resin, 25 parts of organic solvent, 6 parts of emulsifier, 10 parts of antibacterial microcapsules, 12 parts of filler, 1 part of defoamer, and 2 parts of leveling agent; the raw materials of component B are calculated by mass: 30 parts of organic solvent and 25 parts of curing agent.
[0059] The antibacterial coating is prepared by the following method:
[0060] S1) preparing antibacterial microcapsules;
[0061] S11) preparing an emulsified system: adding polyacrylonitrile to deionized water, heating to 60° C., stirring and mixing evenly, adding octenyl succinate starch, stirring at a speed of 500 r / min for 12 min to emulsify, and obtaining a stable emulsified system;
[0062] S12) adding N-(trichloromethyl)-thiophthalimide to the emulsified system at a mass ratio of 1:6.5 of the organic antibacterial agent to polyacrylonitrile, maintaining the temperature at 650° C., and continuing to stir for 15 minutes for coating to obtain antibacterial microcapsules, which were dried and prepared into powder for later use.
[0063] S2) preparing component A and component B respectively;
[0064] S21) Preparation component A:
[0065] S211) Preparation of antibacterial microcapsule dispersion: Weigh antibacterial microcapsules according to the formula ratio, add the antibacterial microcapsules prepared in step S1) into deionized water at a mass ratio of 1:1, stir and mix evenly to obtain an antibacterial microcapsule dispersion:
[0066] S212) adding epoxy resin to an organic solvent according to a formula ratio, stirring and dissolving, then adding sodium dodecyl sulfonate, heating to 70° C., and stirring for 15 minutes to emulsify the epoxy resin to obtain a stable epoxy resin emulsified system; then adding the antibacterial microcapsule dispersion to the epoxy resin emulsified system, and stirring for 25 minutes to mix evenly;
[0067] S213): Add filler, defoamer and leveling agent to component A, stir and mix evenly to obtain component A to be used.
[0068] S22) preparing component B: dissolving the curing agent in an organic solvent to obtain component B.
[0069] S3) adding component B to component A, and stirring and dispersing the component A to obtain coating C for use.
[0070] Example 4
[0071] A sulfuric acid-containing antibacterial paint, with the following formula: the raw materials of component A are calculated by mass: 20 parts of epoxy resin, 30 parts of organic solvent, 2 parts of emulsifier, 5 parts of antibacterial microcapsules, 15 parts of filler, 3 parts of defoamer, and 3 parts of leveling agent; the raw materials of component B are calculated by mass: 40 parts of organic solvent and 25 parts of curing agent.
[0072] The antibacterial coating is prepared by the following method:
[0073] S1) preparing antibacterial microcapsules;
[0074] S11) preparing an emulsified system: adding epoxy resin to deionized water, heating to 50° C., stirring and mixing evenly, adding gum arabic, stirring at a speed of 500 r / min for 15 min to emulsify, and obtaining a stable emulsified system;
[0075] S12) adding 2-bromo-2-nitropropane-1,3-diol to the emulsified system in a mass ratio of 1:5 between the organic antibacterial agent and the epoxy resin, maintaining the temperature at 50° C., and continuing to stir for 20 min for coating to obtain antibacterial microcapsules, which are then dried and prepared into powder for later use.
[0076] S2) preparing component A and component B respectively;
[0077] S21) Preparation component A:
[0078] S211) Preparation of antibacterial microcapsule dispersion: Weigh antibacterial microcapsules according to the formula ratio, add the antibacterial microcapsules prepared in step S1) into deionized water at a mass ratio of 1:1, stir and mix evenly to obtain an antibacterial microcapsule dispersion:
[0079] S212) adding epoxy resin to an organic solvent according to the formula ratio, stirring and dissolving, then adding a multi-block copolymer PEG-(EP-PEG)3-EP-PEG, heating to 60° C., and stirring for 20 minutes to emulsify the epoxy resin to obtain a stable epoxy resin emulsified system; then adding an antibacterial microcapsule dispersion to the epoxy resin emulsified system, and stirring for 30 minutes to mix evenly;
[0080] S213): Add filler, defoamer and leveling agent to component A, stir and mix evenly to obtain component A to be used.
[0081] S22) preparing component B: dissolving the curing agent in an organic solvent to obtain component B.
[0082] S3) Add component B to component A, and stir and disperse them evenly to obtain coating D for use.
[0083] Example 5
[0084] A sulfuric acid-containing antibacterial paint, with the following formula: the raw materials of component A are calculated by mass: 30 parts of epoxy resin, 40 parts of organic solvent, 10 parts of emulsifier, 15 parts of antibacterial microcapsules, 10 parts of filler, 0.5 parts of defoamer, and 1 part of leveling agent; the raw materials of component B are calculated by mass: 50 parts of organic solvent and 40 parts of curing agent.
[0085] The antibacterial coating is prepared by the following method:
[0086] S1) preparing antibacterial microcapsules;
[0087] S11) preparing an emulsified system: adding maltodextrin to deionized water, heating to 70° C., stirring and mixing evenly, adding sucrose ester, stirring at a speed of 500 r / min for 10 min to emulsify, and obtaining a stable emulsified system;
[0088] S12) adding 2-bromo-2-nitropropane-1,3-diol to the emulsified system in a mass ratio of the organic antibacterial agent to maltodextrin of 1:8, maintaining the temperature at 70° C., and continuing to stir for 10 min for coating to obtain antibacterial microcapsules, which are then dried and prepared into powder for later use.
[0089] S2) preparing component A and component B respectively;
[0090] S21) Preparation component A:
[0091] S211) Preparation of antibacterial microcapsule dispersion: Weigh antibacterial microcapsules according to the formula ratio, add the antibacterial microcapsules prepared in step S1) into deionized water at a mass ratio of 1:1, stir and mix evenly to obtain an antibacterial microcapsule dispersion:
[0092] S212) adding epoxy resin to an organic solvent according to a formula ratio, stirring and dissolving, then adding sodium dodecyl sulfonate, raising the temperature to 80° C., and stirring for 10 minutes to emulsify the epoxy resin to obtain a stable epoxy resin emulsified system; then adding the antibacterial microcapsule dispersion to the epoxy resin emulsified system, and stirring for 20 minutes to mix evenly;
[0093] S213): Add filler, defoamer and leveling agent to component A, stir and mix evenly to obtain component A to be used.
[0094] S22) preparing component B: dissolving the curing agent in an organic solvent to obtain component B.
[0095] S3) Add component B to component A, and stir and disperse them evenly to obtain coating E for use.
[0096] Example 6
[0097] A sulfuric acid-containing antibacterial paint, with the following formula: the raw materials of component A are calculated by mass: 25 parts of epoxy resin, 25 parts of organic solvent, 6 parts of emulsifier, 10 parts of antibacterial microcapsules, 12 parts of filler, 1 part of defoamer, and 2 parts of leveling agent; the raw materials of component B are calculated by mass: 30 parts of organic solvent and 25 parts of curing agent.
[0098] The antibacterial coating is prepared by the following method:
[0099] S1) preparing antibacterial microcapsules;
[0100] S11) preparing an emulsified system: adding maltodextrin to deionized water, heating to 60° C., stirring and mixing evenly, adding sucrose ester, stirring at a speed of 500 r / min for 12 min to emulsify the water, and obtaining a stable emulsified system;
[0101] S12) adding 2-bromo-2-nitropropane-1,3-diol to the emulsified system in a mass ratio of the organic antibacterial agent to maltodextrin of 1:6.5, maintaining the temperature at 650° C., and continuing to stir for 15 min for coating to obtain antibacterial microcapsules, which are then dried and prepared into powder for later use.
[0102] S2) preparing component A and component B respectively;
[0103] S21) Preparation component A:
[0104] S211) Preparation of antibacterial microcapsule dispersion: Weigh antibacterial microcapsules according to the formula ratio, add the antibacterial microcapsules prepared in step S1) into deionized water at a mass ratio of 1:1, stir and mix evenly to obtain an antibacterial microcapsule dispersion:
[0105] S212) adding epoxy resin to an organic solvent according to a formula ratio, stirring and dissolving, then adding sodium dodecyl sulfonate, heating to 70° C., and stirring for 15 minutes to emulsify the epoxy resin to obtain a stable epoxy resin emulsified system; then adding the antibacterial microcapsule dispersion to the epoxy resin emulsified system, and stirring for 25 minutes to mix evenly;
[0106] S213): Add filler, defoamer and leveling agent to component A, stir and mix evenly to obtain component A to be used.
[0107] S22) preparing component B: dissolving the curing agent in an organic solvent to obtain component B.
[0108] S3) Add component B to component A, and stir and disperse them evenly to obtain coating F for use.
[0109] Example 7
[0110] A sulfuric acid-containing antibacterial paint, with the following formula: the raw materials of component A are calculated by mass: 25 parts of epoxy resin, 25 parts of organic solvent, 6 parts of emulsifier, 10 parts of antibacterial microcapsules, 12 parts of filler, 1 part of defoamer, and 2 parts of leveling agent; the raw materials of component B are calculated by mass: 30 parts of organic solvent and 25 parts of curing agent.
[0111] The antibacterial coating is prepared by the following method:
[0112] S1) preparing antibacterial microcapsules;
[0113] S11) preparing an emulsified system: adding maltodextrin to deionized water, heating to 60° C., stirring and mixing evenly, adding sucrose ester, stirring at a speed of 500 r / min for 12 min to emulsify the water, and obtaining a stable emulsified system;
[0114] S12) adding 2-bromo-2-nitropropane-1,3-diol and N-(trichloromethyl)-thiophthalimide to an emulsified system in a mass ratio of 1:6.5 of the organic antibacterial agent to maltodextrin, wherein the mass ratio of 2-bromo-2-nitropropane-1,3-diol to N-(trichloromethyl)-thiophthalimide is 3:2, maintaining a constant temperature at 650°C, continuing to stir for 15 minutes for coating, obtaining antibacterial microcapsules, and preparing them into powder after drying for later use.
[0115] S2) preparing component A and component B respectively;
[0116] S21) Preparation component A:
[0117] S211) Preparation of antibacterial microcapsule dispersion: Weigh antibacterial microcapsules according to the formula ratio, add the antibacterial microcapsules prepared in step S1) into deionized water at a mass ratio of 1:1, stir and mix evenly to obtain an antibacterial microcapsule dispersion:
[0118] S212) adding epoxy resin to an organic solvent according to a formula ratio, stirring and dissolving, then adding sodium dodecyl sulfonate, heating to 70° C., and stirring for 15 minutes to emulsify the epoxy resin to obtain a stable epoxy resin emulsified system; then adding the antibacterial microcapsule dispersion to the epoxy resin emulsified system, and stirring for 25 minutes to mix evenly;
[0119] S213): Add filler, defoamer and leveling agent to component A, stir and mix evenly to obtain component A to be used.
[0120] S22) preparing component B: dissolving the curing agent in an organic solvent to obtain component B.
[0121] S3) Add component B to component A, and stir and disperse them evenly to obtain coating G for use.
[0122] The coatings prepared above were coated on metal plates respectively, and after curing, a coating with a thickness of 0.5 mm was formed. The acid resistance was tested by 0.05 mol / L dilute sulfuric acid and 0.1 mol / L dilute hydrochloric acid. The antibacterial rate was tested after immersion in oil and gas field produced water for 30 days and 150 days. The test results are as follows:
[0123]
[0124] It can be seen that the coating disclosed in the present invention has good acid resistance and good and lasting antibacterial property.
[0125] The above shows and describes the basic principles, main features and advantages of the present invention, so the above is only an embodiment of the present invention. It should be understood by those skilled in the art that the present invention is not limited by the above embodiments, and the above embodiments and descriptions only describe the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention also includes various equivalent changes and improvements, which will fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. An antibacterial coating for sulfuric acid-containing petroleum and natural gas environments, characterized in that The invention comprises component A and component B, wherein component A comprises epoxy resin, organic solvent, emulsifier and antibacterial microcapsule; component B comprises organic solvent and curing agent; the antibacterial microcapsule takes organic antibacterial agent as core material and takes any one of maltodextrin, alginate, epoxy resin or polyacrylonitrile as shell material; the raw materials of component A are calculated by mass as follows: 20-30 parts of epoxy resin, 25-40 parts of organic solvent, 2-10 parts of emulsifier and 5-15 parts of antibacterial microcapsule; the raw materials of component B are calculated by mass as follows: 30-50 parts of organic solvent and 25-40 parts of curing agent; the organic antibacterial agent is N-(trichloromethyl)-thiophthalimide and / or 2-bromo-2-nitropropane-1,3-diol, and the emulsifier comprises one or more of OP-10, sodium dodecyl sulfonate and multi-block copolymer PEG-(EP-PEG)3-EP-PEG.
2. The coating according to claim 1, characterized in that The embedding rate of the organic antibacterial agent in the microcapsule is not less than 10%.
3. The coating according to claim 1, characterized in that The component A further comprises a filler, a defoamer and a leveling agent. The filler accounts for 10 to 15 parts by mass; the defoamer accounts for 0.5 to 3 parts by mass; and the leveling agent accounts for 1 to 3 parts by mass.
4. The coating according to claim 1, characterized in that The curing agent is one or more of phenolic resin, polyamide and aliphatic polyamine.
5. The method for preparing an antibacterial coating for sulfuric acid-containing petroleum and natural gas environments according to any one of claims 1-2 and 4, characterized in that The following steps are involved: S1) preparing antibacterial microcapsules; S2) preparing component A and component B respectively; S3) Add component B to component A, and stir and disperse them evenly to obtain the coating.
6. The method according to claim 5, characterized in that Step S1) comprises the following steps: S11) preparing an emulsified system: adding the shell material to deionized water, heating to 50-70° C., stirring and mixing evenly, adding a shell material emulsifier, stirring and emulsifying, and obtaining a stable emulsified system; S12) adding an organic antibacterial agent to the emulsified system, maintaining a constant temperature, and continuously stirring to coat the system to obtain antibacterial microcapsules, which are then dried and prepared into powder for later use.
7. The method according to claim 5, characterized in that The shell material emulsifier is one or any two of octenyl succinate starch ester, sucrose ester, monoglyceride, carrageenan, modified starch and gum arabic.
8. The method according to claim 5, characterized in that Step S2) comprises the following steps: S21) Preparation component A: S211) Preparation of antibacterial microcapsule dispersion: Add the antibacterial microcapsules prepared in step S1) into deionized water, stir and mix evenly to obtain an antibacterial microcapsule dispersion: S212) adding epoxy resin to an organic solvent, stirring and dissolving, then adding an emulsifier, heating to 60-80° C., and continuing to stir to emulsify, to obtain a stable epoxy resin emulsified system; then adding an antibacterial microcapsule dispersion to the epoxy resin emulsified system, continuing to stir and mix evenly, to obtain component A; S22) preparing component B: dissolving the curing agent in an organic solvent to obtain component B.
9. The method according to claim 8, characterized in that Step S21) also includes S213): adding filler, defoamer and leveling agent into component A, stirring and mixing evenly to obtain component A to be used.
Citation Information
Patent Citations
Phase change microcapsule and preparation method thereof
CN104096521A
Paint with long-acting anti-microbial properties and preparation method thereof
CN106978033A
Self-repairing anticorrosive coating and preparation method thereof
CN111205745A