Sodium supplement material and preparation method thereof, positive electrode sheet, electrode assembly, battery and electrical device
By using the cladding of lattice oxygen-stabilized materials and oxygen adsorption materials in sodium supplementary materials, the problems of sodium loss and excessive oxygen release in sodium secondary batteries are solved, and the battery performance and cycle life are significantly improved.
Patent Information
- Application Number
- CN202310897810.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-07-21
AI Technical Summary
There is a problem of sodium loss during the circulation of sodium secondary batteries, which leads to excessive oxygen release, affecting battery performance and cycle life.
A sodium supplement material is used, which includes a sodium supplement agent and a coating layer provided on the surface of the sodium supplement agent. The coating layer includes a lattice oxygen-stabilized material and/or an oxygen adsorption material to stabilize the sodium supplement through the lattice oxygen-stabilized material. The surface structure of the agent inhibits the detachment of lattice oxygen, and adsorbs or consumes released oxygen through the oxygen adsorption layer, reducing the entry of oxygen into the electrolyte.
Effectively reduce the amount of oxygen released, improve the stability of sodium supplementary materials, reduce the entry of oxygen into the electrolyte, and improve battery performance and cycle life.
Smart Images

Figure CN116632220B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery technology, and in particular to a sodium supplement material and a preparation method thereof, a positive electrode sheet, an electrode assembly, a battery and an electrical device. Background Art
[0002] Sodium secondary batteries have great development prospects in the field of large-scale energy storage due to their abundant sodium reserves.
[0003] There is a problem of sodium loss during the cycling of sodium secondary batteries. Summary of the Invention
[0004] The main purpose of the present invention is to provide a sodium supplement material to improve the performance of the battery.
[0005] To achieve the above objectives, the present invention provides a sodium supplement material, which includes a sodium supplement agent and a coating layer provided on the surface of the sodium supplement agent, wherein the coating layer includes a lattice oxygen stabilizing material and / or an oxygen adsorbing material.
[0006] Considering that lattice oxygen will escape from the sodium supplement material during the sodium supplement process and react with the electrolyte to produce oxygen. In order to improve gas production, the sodium supplement material includes a sodium supplement agent and a coating layer provided on the surface of the sodium supplement agent, and the coating layer includes a lattice oxygen stabilizing material and / or an oxygen adsorbing material. The lattice oxygen stabilizing material can stabilize the surface structure of the sodium supplement agent, inhibit the escape of lattice oxygen, and reduce the amount of oxygen released. The oxygen adsorbing layer can adsorb and / or react with the released oxygen, reducing the entry of oxygen into the electrolyte. The lattice oxygen stabilizing material and / or the oxygen adsorbing material can improve the release of oxygen in the sodium supplement material and improve the performance of the battery.
[0007] It is understood that the coating layer can be a single-layer structure or a multi-layer structure. For example, in a single-layer structure, the coating layer includes a lattice oxygen-stabilizing material or an oxygen-absorbing material, or the coating layer includes both a lattice oxygen-stabilizing material and an oxygen-absorbing material. In a multi-layer structure, at least one layer can include a lattice oxygen-stabilizing material and at least one layer can include an oxygen-absorbing material. For example, in one embodiment, the coating layer has a two-layer structure, one layer including a lattice oxygen-stabilizing material and the other including an oxygen-absorbing material. Those skilled in the art can configure the structure according to actual needs.
[0008] Optionally, the coating layer includes a lattice oxygen stabilization layer and an oxygen adsorption layer, the lattice oxygen stabilization layer is provided on the surface of the sodium supplement, and the oxygen adsorption layer is provided on the surface of the lattice oxygen stabilization layer;
[0009] The lattice oxygen stabilizing layer includes a lattice oxygen stabilizing material, and the oxygen adsorption layer includes an oxygen adsorption material.
[0010] In order to effectively improve the release of oxygen in the sodium supplement material, the coating layer includes a lattice oxygen stabilization layer and an oxygen adsorption layer. The lattice oxygen stabilization layer includes a lattice oxygen stabilization material, and the oxygen adsorption layer includes an oxygen adsorption material. The lattice oxygen stabilization layer is arranged on the surface of the sodium supplement agent, so that the lattice oxygen stabilization layer is arranged close to the sodium supplement agent, which can block the contact between the sodium supplement agent and the electrolyte, effectively improve the stability of the sodium supplement agent structure, and improve the escape of lattice oxygen. The oxygen adsorption layer is arranged on the surface of the lattice oxygen stabilization layer, so that the escaped oxygen can pass through the oxygen adsorption layer and be filtered, thereby reducing the oxygen entering the electrolyte.
[0011] Optionally, the lattice oxygen stabilization layer completely covers the surface of the sodium supplement;
[0012] And / or, the oxygen adsorption layer completely covers the surface of the lattice oxygen stabilization layer.
[0013] Considering that direct contact between the sodium supplementer and the electrolyte will produce side reactions and accelerate the release of lattice oxygen, in order to improve the release of lattice oxygen, the lattice oxygen stabilization layer is fully coated on the surface of the sodium supplementer to block direct contact between the sodium supplementer and the electrolyte, thereby improving the release of lattice oxygen.
[0014] The oxygen adsorption layer is fully coated on the surface of the lattice oxygen stabilization layer, so that the released oxygen passes through the oxygen adsorption layer, which helps the oxygen adsorption layer to filter the released oxygen.
[0015] Optionally, the lattice oxygen stabilizing material includes at least one of transition metal oxides, sulfides, phosphates, and conductive polymers.
[0016] Transition metal oxides, sulfides, phosphates, conductive polymers, etc. can form a physical barrier layer on the surface of the sodium supplementer, reduce the contact between the sodium supplementer and the electrolyte, improve the side reactions between the residual sodium salts and alkaline substances on the surface of the sodium supplementer and the electrolyte, thereby reducing the chemical erosion of the sodium supplementer by by-products, stabilizing the material structure of the sodium supplementer, and improving the release of lattice oxygen.
[0017] It is understood that the lattice oxygen stabilizing material includes but is not limited to at least one of transition metal oxides, sulfides, phosphates, and conductive polymers. For example, the lattice oxygen stabilizing material can be one of transition metal oxides, sulfides, phosphates, and conductive polymers, or a composite of multiple materials. It is understood that the composite of transition metal oxides with at least one of sulfides, phosphates, and conductive polymers is better than the composite of two of sulfides, phosphates, and conductive polymers. For example, due to the different electrochemical properties of the coating materials, the conductivity of a single coating material will deteriorate, and the composite material can improve the electronic and ionic conductivity of the coating material while coating; for example, due to the different physical properties of the coating materials, the coating layer formed by a single coating material may be a point-shaped or island-shaped coating, and the composite coating can form a uniform and dense coating layer, which can better play a physical barrier role.
[0018] Optionally, the transition metal oxide includes at least one of V2O5, ZrO2, TiO2, RuO2, La2O3, and CeO2;
[0019] And / or, the sulfide includes at least one of titanium disulfide, iron sulfide, cobalt sulfide, nickel sulfide, molybdenum sulfide, tin sulfide, and antimony sulfide;
[0020] And / or, the phosphate includes at least one of titanium phosphate, titanium pyrophosphate, sodium titanium phosphate, sodium titanium aluminum phosphate, and sodium vanadium phosphate;
[0021] And / or, the conductive polymer includes at least one of polypyrrole, polyethylene glycol, polyaniline, and poly(3,4-ethylenedioxythiophene).
[0022] The transition metal oxides in this application include but are not limited to at least one of V2O5, ZrO2, TiO2, RuO2, La2O3, and CeO2.
[0023] The sulfide includes, but is not limited to, at least one of titanium disulfide, iron sulfide, cobalt sulfide, nickel sulfide, molybdenum sulfide, tin sulfide, and antimony sulfide.
[0024] The conductive polymer includes, but is not limited to, at least one of polypyrrole, polyethylene glycol, polyaniline, and poly(3,4-ethylenedioxythiophene).
[0025] Optionally, the oxygen adsorption material includes at least one of a porous oxygen absorbing material and an organic oxygen absorbing material.
[0026] The oxygen absorbing material includes, but is not limited to, at least one of a porous oxygen absorbing material and an organic oxygen absorbing material. The oxygen absorbing material can absorb oxygen through physical adsorption to improve oxygen release, or directly consume oxygen through a chemical reaction to improve oxygen release.
[0027] Optionally, the porous oxygen absorbing material includes at least one of activated carbon, carbon molecular sieve, zeolite molecular sieve, and silicon titanium molecular sieve;
[0028] And / or, the organic oxygen-absorbing material includes at least one of a phenolic antioxidant, an amine antioxidant, and a phosphite antioxidant.
[0029] Porous oxygen-absorbing materials include, but are not limited to, at least one of activated carbon, carbon molecular sieves, zeolite molecular sieves, and silicon-titanium molecular sieves. These materials are porous and can act as adsorbents to absorb both lattice oxygen and oxygen. It is understood that lattice oxygen released from the sodium supplement reaches the porous oxygen-absorbing material and is also adsorbed within its pores. Organic oxygen-absorbing materials include, but are not limited to, at least one of phenolic antioxidants, amine antioxidants, and phosphite antioxidants. These antioxidants react chemically with oxygen, oxidizing the antioxidant itself into products that have no adverse effects on the battery cell while consuming oxygen, thereby improving oxygen release.
[0030] Optionally, the phenolic antioxidant includes at least one of butylated hydroxyanisole, butylated hydroxytoluene, propyl gallate, and tert-butylhydroquinone;
[0031] And / or, the amine antioxidant includes at least one of naphthylamine, diphenylamine, and p-phenylenediamine;
[0032] And / or, the phosphite antioxidant includes at least one of bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, tris(2,4-di-tert-butylphenyl)phosphite, bis[2-methyl-4,6-bis(1,1'-dimethylethyl)phenol]ethyl phosphate, tetrakis(2,4-di-tert-butyloctaalkoxy-4,4-biphenyl)phosphate, (2,4,6-tri-tert-butylphenyl-2-butyl-2-ethyl)-1,3-propylene glycol phosphite, and di(2,4-di-p-isopropylphenyl)pentaerythritol diphosphite.
[0033] The phenolic antioxidants in the present application include, but are not limited to, at least one of butylated hydroxyanisole, butylated hydroxytoluene, propyl gallate, and tert-butylhydroquinone.
[0034] The amine antioxidant includes but is not limited to at least one of naphthylamine, diphenylamine, and p-phenylenediamine.
[0035] Phosphite antioxidants include, but are not limited to, at least one of bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, tris(2,4-di-tert-butylphenyl)phosphite, bis[2-methyl-4,6-bis(1,1-dimethylethyl)phenol]ethyl phosphate, tetrakis(2,4-di-tert-butyloctaalkoxy-4,4-biphenyl)phosphate, (2,4,6-tri-tert-butylphenyl-2-butyl-2-ethyl)-1,3-propylene glycol phosphite, and di(2,4-di-p-isopropylphenyl)pentaerythritol diphosphite.
[0036] Optionally, the Dv50 value of the sodium supplement material is in the range of greater than 1 μm and less than or equal to 30 μm.
[0037] Optionally, the Dv50 value of the sodium supplement material ranges from 5 μm to 25 μm.
[0038] Sodium-supplementing materials are used in the positive electrode coating to improve sodium loss during the cycle. Sodium-supplementing materials need to be mixed with the positive electrode material. The Dv50 of the sodium-supplementing material is within the above range, which can improve the coating process, for example, improve the gel and improve the problem of uneven distribution of the sodium-supplementing material. It is understandable that while maintaining the mass of the sodium-supplementing material unchanged, the number of particles of the sodium-supplementing material will decrease when the size of the sodium-supplementing material gradually increases, resulting in uneven distribution of the sodium-supplementing material in the active layer. When the size of the sodium-supplementing material is small, the sodium-supplementing material is prone to agglomeration. The above phenomenon will result in a higher capacity of the coating area with the sodium-supplementing material. During the sodium removal process, sodium may be precipitated at the negative electrode, which places higher requirements on the capacity of the negative electrode. To this end, setting the Dv50 of the sodium-supplementing material within the above range can alleviate the above problems.
[0039] Optionally, the coating layer has a thickness ranging from 10 nm to 1000 nm.
[0040] Optionally, the coating layer has a thickness ranging from 100 nm to 800 nm.
[0041] It can be understood that the thickness of the coating layer is within the above range, which can improve the escape of lattice oxygen and the release of oxygen. At the same time, considering that the coating layer includes materials with poor conductivity, setting the thickness of the coating layer within the above range can improve the escape of sodium and improve the sodium supplementation effect.
[0042] Optionally, the thickness of the lattice oxygen stabilization layer is in a range of 10 nm to 400 nm;
[0043] And / or, the thickness of the oxygen adsorption layer ranges from 10 nm to 600 nm.
[0044] Optionally, the thickness of the lattice oxygen stabilization layer is in a range of 50 nm to 300 nm;
[0045] And / or, the thickness of the oxygen adsorption layer is in the range of 50 nm to 500 nm.
[0046] When the thickness of the lattice oxygen stabilizing layer is within the above range, the release of lattice oxygen can be improved.
[0047] The thickness of the oxygen adsorption layer is within the above range, which can improve the adsorption and consumption of oxygen, thereby reducing the amount of oxygen entering the electrolyte.
[0048] Optionally, the ratio of the Dv50 of the sodium supplement to the Dv50 of the oxygen adsorbent is 5:1 to 250:1, and the oxygen adsorbent comprises a porous oxygen absorbing material;
[0049] and / or, the sodium supplement has a Dv50 value ranging from 1 μm to 25 μm;
[0050] And / or, the Dv50 value of the oxygen adsorbing material is in the range of 10 nm to 200 nm, and the oxygen adsorbing material comprises a porous oxygen absorbing material.
[0051] Considering that when the porous oxygen-absorbing material is coated on the surface of the sodium supplementer, it is difficult to effectively coat the surface of the sodium supplementer if the particle size of the porous oxygen-absorbing material is too large, the ratio of the Dv50 of the sodium supplementer to the Dv50 of the oxygen adsorption material is set within the above range so that the porous oxygen-absorbing material can be effectively coated on the surface of the sodium supplementer.
[0052] The Dv50 of the sodium supplement agent is within the above range, which helps to obtain sodium supplement materials of appropriate size and facilitates the coating process operation after the sodium supplement material is mixed with the positive electrode material.
[0053] The Dv50 of the porous oxygen absorbing material is within the above range, so that the porous oxygen absorbing material can be effectively coated on the surface of the sodium supplement agent.
[0054] Optionally, the chemical formula of the sodium supplement includes Na x1 MO2 and / or Na x2 MO4, 2≤x1<4, 2≤x2<8, M includes at least one of Ni, Co, Mn, Al, Zr, Ti, V, Er, Ca, Fe, Ru, Ir, Sn, Cr, Cu, Nb, and Mo.
[0055] The chemical formula of the sodium supplement of the present application includes but is not limited to Na x1 MO2 and / or Na x2 MO4, 2≤x1<4, 2≤x2<8, M includes at least one of Ni, Co, Mn, Al, Zr, Ti, V, Er, Ca, Fe, Ru, Ir, Sn, Cr, Cu, Nb, and Mo.
[0056] The present application also provides a method for preparing a sodium supplement material, comprising:
[0057] Prepare sodium supplements;
[0058] The sodium supplementing agent is mixed with a lattice oxygen stabilizing material, and calcined to obtain the sodium supplementing material, so that the lattice oxygen stabilizing material forms a coating layer on the surface of the sodium supplementing agent, wherein the sodium supplementing material obtained by calcination comprises the sodium supplementing agent and the coating layer provided on the surface of the sodium supplementing agent, and the coating layer comprises the lattice oxygen stabilizing material;
[0059] Alternatively, the method for preparing the sodium supplementing material comprises:
[0060] Prepare sodium supplements;
[0061] The sodium supplementing agent and the oxygen adsorbing material are placed in a solvent and mixed, and dried to obtain the sodium supplementing material, so that the oxygen adsorbing material forms a coating layer on the surface of the sodium supplementing agent, the sodium supplementing material comprises the sodium supplementing agent and the coating layer provided on the surface of the sodium supplementing agent, and the coating layer comprises the oxygen adsorbing material;
[0062] Alternatively, the method for preparing the sodium supplementing material comprises:
[0063] Prepare sodium supplements;
[0064] Mixing the sodium supplement agent with a lattice oxygen stabilizing material, and calcining to obtain a material, so that the lattice oxygen stabilizing material is coated on the surface of the sodium supplement agent;
[0065] The calcined material is placed in a solvent and mixed with an oxygen adsorbing material, and dried to obtain a sodium supplementing material, so that the lattice oxygen stabilizing material and the oxygen adsorbing material form a coating layer on the surface of the sodium supplementing agent. The sodium supplementing material includes a sodium supplementing agent and the coating layer provided on the surface of the sodium supplementing agent, and the coating layer includes the lattice oxygen stabilizing material and the oxygen adsorbing material.
[0066] The present application obtains a sodium-supplementing material having a sodium-supplementing agent coated with a lattice oxygen-stabilizing material by mixing the sodium-supplementing agent with the lattice oxygen-stabilizing material and calcining the mixture.
[0067] The present application prepares a sodium supplementing material in which the sodium supplementing agent is coated with the oxygen adsorbing material by mixing the sodium supplementing agent with the oxygen adsorbing material in a solvent and drying the mixture.
[0068] The present application obtains a sodium-supplementing material by mixing a sodium-supplementing agent with a lattice oxygen-stabilizing material, calcining the mixture, mixing the calcined material with an oxygen adsorption material in a solvent, and drying the mixture. The coating layer of the sodium-supplementing material includes the lattice oxygen-stabilizing material and the oxygen adsorption material.
[0069] Optionally, the process of preparing the sodium supplement includes the following steps:
[0070] A sodium source and a metal source are mixed and calcined to obtain a sodium supplement agent, wherein the calcination temperature is 500° C. to 1200° C. and the calcination time is 3 h to 12 h.
[0071] The sodium supplementer of the present application can be directly a commercial material or can be directly prepared from raw materials. During the preparation process, a sodium source and a metal source are mixed and calcined to obtain the sodium supplementer, wherein the calcination temperature is 500° C. to 1200° C. and the calcination time is 3 h to 12 h.
[0072] Optionally, in the step of mixing the sodium supplement with a lattice oxygen stabilizing material and calcining to obtain the material, the lattice oxygen stabilizing material includes at least one of a transition metal oxide, a sulfide, and a phosphate, the calcination temperature is 200°C to 600°C, and the calcination time is 2h to 8h.
[0073] In the step of mixing the sodium supplement with the lattice oxygen stabilizing material and calcining to obtain the material, the lattice oxygen stabilizing material includes at least one of a transition metal oxide, a sulfide, and a phosphate, the calcination temperature is 200° C. to 600° C., and the calcination time is 2 h to 8 h.
[0074] Optionally, in the step of mixing the sodium supplement with a lattice oxygen-stabilizing material and calcining to obtain a material, the lattice oxygen-stabilizing material includes a conductive polymer, the calcination temperature is 150° C. to 450° C., and the calcination time is 2 h to 8 h.
[0075] Optionally, the sodium source includes at least one of sodium oxide, sodium hydroxide, sodium peroxide, sodium carbonate, sodium bicarbonate, sodium sulfate, sodium phosphate, sodium nitrate, sodium acetate, sodium chloride or sodium fluoride;
[0076] And / or, the mass ratio of the sodium supplement to the lattice oxygen stabilizing material is in a range of 1% to 10%;
[0077] And / or, the mass ratio of the sodium supplement to the oxygen adsorbent is in a range of 1% to 10%;
[0078] and / or, the ratio of the Dv50 of the sodium supplement to the Dv50 of the oxygen adsorbent is 5:1 to 250:1, and the oxygen adsorbent comprises a porous oxygen-absorbing material;
[0079] And / or, the solvent includes at least one of ethanol, ethylene glycol, diethylene glycol, and polyethylene glycol 400.
[0080] The sodium source of the present application includes but is not limited to at least one of sodium oxide, sodium hydroxide, sodium peroxide, sodium carbonate, sodium bicarbonate, sodium sulfate, sodium phosphate, sodium nitrate, sodium acetate, sodium chloride or sodium fluoride.
[0081] The mass ratio of the sodium supplement to the lattice oxygen stabilizing material is within the above range, and the thickness of the lattice oxygen stabilizing layer can be obtained in the range of 1 nm to 50 nm.
[0082] The mass ratio of the sodium supplement to the oxygen adsorption material is within the above range, and the thickness of the oxygen adsorption layer can be in the range of 10 nm to 600 nm.
[0083] The ratio of the Dv50 of the sodium supplementer to the Dv50 of the porous oxygen absorbing material is within the above range, which can effectively coat the porous adsorption material on the surface of the sodium supplementer.
[0084] The solvent in the present application includes but is not limited to at least one of ethanol, ethylene glycol, diethylene glycol, and polyethylene glycol 400.
[0085] The present application also provides a positive electrode plate, the positive electrode plate comprising the sodium supplement material as described above;
[0086] Alternatively, the positive electrode plate includes the sodium-supplementing material obtained by the preparation method of the sodium-supplementing material.
[0087] Optionally, the positive electrode plate includes an active material, and the mass of the sodium-supplementing material accounts for a percentage greater than 0 and less than or equal to 20% of the total mass of the active material and the sodium-supplementing material.
[0088] Optionally, the mass of the sodium-supplementing material accounts for 5% to 15% of the total mass of the active material and the sodium-supplementing material.
[0089] The loss of sodium ions leads to very low first-cycle efficiency in sodium-ion batteries, ranging from approximately 50% to 85%. Adjusting the mass percentage of the sodium-supplementing material to the total mass of the active material and the sodium-supplementing material within this range can compensate for this loss and improve battery performance. It is understood that if the mass percentage of the sodium-supplementing material to the total mass of the active material and the sodium-supplementing material is too large, the amount of active material used will be reduced. Given that the performance of the sodium-supplementing material is inferior to that of the active material, increasing the amount of the sodium-supplementing material in this situation will reduce battery performance.
[0090] The present application also provides an electrode assembly, which includes a negative electrode plate, an electrolyte, and a positive electrode plate as described above.
[0091] The present application also provides a battery, which includes the electrode assembly as described above.
[0092] The present application also provides an electrical device, which includes the battery as described above.
[0093] The sodium-supplementing material of the present application includes a sodium-supplementing agent and a coating disposed on the surface of the sodium-supplementing agent. The coating includes a lattice oxygen-stabilizing material and / or an oxygen-adsorbing material. The lattice oxygen-stabilizing material can stabilize the structure of the sodium-supplementing agent, improve the release of lattice oxygen, and reduce the amount of oxygen released. The oxygen-adsorbing layer can filter the released oxygen and reduce the amount of oxygen entering the electrolyte. The lattice oxygen-stabilizing material and / or the oxygen-adsorbing material can improve the release of oxygen from the sodium-supplementing material and improve the performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0094] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.
[0095] Figure 1 Schematic diagram of the structure of a sodium supplement material according to one embodiment of the present application;
[0096] Figure 2 Schematic diagram of the structure of a sodium supplement material according to another embodiment of the present application;
[0097] Figure 3 This is a flow chart of the preparation process of the sodium supplement material according to one embodiment of the present application;
[0098] Figure 4 is a schematic diagram of a battery cell according to one embodiment of the present application;
[0099] Figure 5 yes Figure 4 An exploded view of a battery cell according to an embodiment of the present application is shown;
[0100] Figure 6 is a schematic diagram of a battery module according to one embodiment of the present application;
[0101] Figure 7 is a schematic diagram of a battery pack according to one embodiment of the present application;
[0102] Figure 8 yes Figure 7 An exploded view of a battery pack according to an embodiment of the present application is shown;
[0103] Figure 9 FIG2 is a schematic diagram of an electrical device using a battery cell according to an embodiment of the present application as a power source.
[0104] Description of Figure Numbers:
[0105]
[0106] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings and in conjunction with the embodiments. DETAILED DESCRIPTION
[0107] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making any creative efforts shall fall within the scope of protection of the present invention.
[0108] Below, the sodium supplement material and its preparation method, positive electrode plate, electrode assembly, battery and electric device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0109] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0110] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0111] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0112] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0113] There is a problem of sodium loss during the cycling of sodium secondary batteries.
[0114] Sodium supplements are usually used to replace sodium losses.
[0115] However, there are some problems in the process of supplementing sodium with sodium supplements.
[0116] For example, during the sodium removal process, lattice oxygen will be released and react with the electrolyte to produce oxygen, which will be released from the anode, resulting in large gas production during the formation process, causing unstable film formation, abnormal interface and affecting the subsequent cycle life. Although most of the gas will be extracted during the negative pressure formation process, some active oxygen will still remain in the electrolyte, gradually oxidizing the electrolyte, causing excessive gas production in the battery cell in the later stage, and the battery cell valve will open to spray liquid.
[0117] In order to improve the above problems, the present application provides a sodium supplement material, which includes a sodium supplement agent and a coating layer provided on the surface of the sodium supplement agent, wherein the coating layer includes a lattice oxygen stabilizing material and / or an oxygen adsorption material.
[0118] Sodium supplement materials, including metal oxides of sodium, can irreversibly release one or more sodium ions in secondary batteries to supplement the sodium loss of the secondary battery during the first cycle of charging and film formation and subsequent cycles.
[0119] Coating, such as Figure 1 As shown, a coating layer 20 is provided on the surface of the sodium supplementing agent 10 , and the coating layer 20 coats the surface of the sodium supplementing agent 10 .
[0120] Lattice oxygen, the bulk oxygen that constitutes the crystal structure, such as the oxygen that constitutes the anatase structure in TiO2.
[0121] Lattice oxygen stabilizing materials improve the stability of sodium supplement materials through physical effects and improve the release of lattice oxygen in sodium supplement agents.
[0122] Oxygen adsorption materials improve the release of oxygen into the electrolyte by physically adsorbing oxygen or consuming oxygen through chemical reactions.
[0123] Considering that lattice oxygen will escape from the sodium supplement material during the sodium supplement process and react with the electrolyte to produce oxygen. In order to improve gas production, the sodium supplement material includes a sodium supplement agent and a coating layer provided on the surface of the sodium supplement agent, and the coating layer includes a lattice oxygen stabilizing material and / or an oxygen adsorbing material. The lattice oxygen stabilizing material can stabilize the surface structure of the sodium supplement agent, inhibit the escape of lattice oxygen, and reduce the amount of oxygen released. The oxygen adsorbing layer can adsorb and / or react with the released oxygen, reducing the entry of oxygen into the electrolyte. The lattice oxygen stabilizing material and / or the oxygen adsorbing material can improve the release of oxygen in the sodium supplement material and improve the performance of the battery.
[0124] Therefore, by providing a coating layer on the surface of the sodium supplement, the release of oxygen can be improved, thereby improving the performance of the battery.
[0125] It is understood that the coating layer can be a single layer structure, for example Figure 1 As shown, it can also be a multi-layer structure, such as Figure 2 As shown, the surface of the sodium supplement 10 is provided with a lattice oxygen stabilization layer 21, and the surface of the lattice oxygen stabilization layer 21 is provided with an oxygen adsorption layer 22. For example, in a single-layer structure, the coating layer includes a lattice oxygen stabilization material or an oxygen adsorption material, or the coating layer includes both a lattice oxygen stabilization material and an oxygen adsorption material. In a multi-layer structure, at least one layer may include a lattice oxygen stabilization material and at least one layer may include an oxygen adsorption material. For example, a two-layer structure may include one layer including a lattice oxygen stabilization material and the other layer including an oxygen adsorption material. Those skilled in the art can make the configuration according to actual needs.
[0126] In one embodiment, the coating layer includes a lattice oxygen stabilization layer and an oxygen adsorption layer. The lattice oxygen stabilization layer is arranged on the surface of the sodium supplementer, and the oxygen adsorption layer is arranged on the surface of the lattice oxygen stabilization layer; the lattice oxygen stabilization layer includes a lattice oxygen stabilization material, and the oxygen adsorption layer includes an oxygen adsorption material.
[0127] like Figure 2 As shown, the coating layer includes at least two layers, the lattice oxygen stabilization layer is arranged on the surface of the sodium supplementer, and the oxygen adsorption layer is arranged on the surface of the lattice oxygen stabilization layer; the lattice oxygen stabilization layer includes a lattice oxygen stabilization material, and the oxygen adsorption layer includes an oxygen adsorption material.
[0128] In order to effectively improve the release of oxygen in the sodium supplement material, the coating layer includes a lattice oxygen stabilization layer and an oxygen adsorption layer. The lattice oxygen stabilization layer includes a lattice oxygen stabilization material, and the oxygen adsorption layer includes an oxygen adsorption material. The lattice oxygen stabilization layer is arranged on the surface of the sodium supplement agent, so that the lattice oxygen stabilization layer is arranged close to the sodium supplement agent, which can block the contact between the sodium supplement agent and the electrolyte, effectively improve the stability of the sodium supplement agent structure, and improve the escape of lattice oxygen. The oxygen adsorption layer is arranged on the surface of the lattice oxygen stabilization layer, so that the escaped oxygen can pass through the oxygen adsorption layer and be filtered, thereby reducing the oxygen entering the electrolyte.
[0129] In one embodiment, the lattice oxygen stabilization layer completely covers the surface of the sodium supplement agent; and / or the oxygen adsorption layer completely covers the surface of the lattice oxygen stabilization layer.
[0130] Full coating means that the coating material is continuously coated on the surface of the sodium supplement agent to prevent the surface of the sodium supplement agent from being exposed.
[0131] Considering that direct contact between the sodium supplementer and the electrolyte will produce side reactions and accelerate the release of lattice oxygen, in order to improve the release of lattice oxygen, the lattice oxygen stabilization layer is fully coated on the surface of the sodium supplementer to block direct contact between the sodium supplementer and the electrolyte, thereby improving the release of lattice oxygen.
[0132] The oxygen adsorption layer is fully coated on the surface of the lattice oxygen stabilization layer, so that the released oxygen passes through the oxygen adsorption layer, which helps the oxygen adsorption layer to filter the released oxygen.
[0133] In one embodiment, the lattice oxygen stabilizing material includes at least one of a transition metal oxide, a sulfide, a phosphate, and a conductive polymer.
[0134] Transition metal oxides, sulfides, phosphates, conductive polymers, etc. can form a physical barrier layer on the surface of the sodium supplementer, reduce the contact between the sodium supplementer and the electrolyte, improve the side reactions between the residual sodium salts and alkaline substances on the surface of the sodium supplementer and the electrolyte, thereby reducing the chemical erosion of the sodium supplementer by by-products, stabilizing the material structure of the sodium supplementer, and improving the release of lattice oxygen.
[0135] It is understood that the lattice oxygen stabilizing material includes but is not limited to at least one of transition metal oxides, sulfides, phosphates, and conductive polymers. For example, the lattice oxygen stabilizing material can be one of transition metal oxides, sulfides, phosphates, and conductive polymers, or a composite of multiple materials. It is understood that the composite of transition metal oxides with at least one of sulfides, phosphates, and conductive polymers is better than the composite of two of sulfides, phosphates, and conductive polymers. For example, due to the different electrochemical properties of the coating materials, the conductivity of a single coating material will deteriorate, and the composite material can improve the electronic and ionic conductivity of the coating material while coating; for example, due to the different physical properties of the coating materials, the coating layer formed by a single coating material may be a point-shaped or island-shaped coating, and the composite coating can form a uniform and dense coating layer, which can better play a physical barrier role.
[0136] In one embodiment, the transition metal oxide includes at least one of V2O5, ZrO2, TiO2, RuO2, La2O3, and CeO2; and / or the sulfide includes at least one of titanium disulfide, iron sulfide, cobalt sulfide, nickel sulfide, molybdenum sulfide, tin sulfide, and antimony sulfide; and / or the phosphate includes at least one of titanium phosphate, titanium pyrophosphate, sodium titanium phosphate, sodium titanium aluminum phosphate, and sodium vanadium phosphate; and / or the conductive polymer includes at least one of polypyrrole, polyethylene glycol, polyaniline, and poly(3,4-ethylenedioxythiophene).
[0137] Transition metal oxides, oxides containing transition metals.
[0138] Conductive polymers, polymers themselves have the ability to transport charges.
[0139] In this application, transition metal oxides include, but are not limited to, at least one of V2O5, ZrO2, TiO2, RuO2, La2O3, and CeO2. Sulfides include, but are not limited to, at least one of titanium disulfide, iron sulfide, cobalt sulfide, nickel sulfide, molybdenum sulfide, tin sulfide, and antimony sulfide. Conductive polymers include, but are not limited to, at least one of polypyrrole, polyethylene glycol, polyaniline, and poly(3,4-ethylenedioxythiophene).
[0140] In one embodiment, the oxygen absorbing material includes at least one of a porous oxygen absorbing material and an organic oxygen absorbing material.
[0141] Porous oxygen-absorbing materials have a porous structure and can absorb oxygen.
[0142] Organic oxygen-absorbing materials are organic substances that can absorb and consume oxygen.
[0143] The oxygen absorbing material includes, but is not limited to, at least one of a porous oxygen absorbing material and an organic oxygen absorbing material. The oxygen absorbing material can absorb oxygen through physical adsorption to improve oxygen release, or directly consume oxygen through a chemical reaction to improve oxygen release.
[0144] In one embodiment, the porous oxygen-absorbing material includes at least one of activated carbon, carbon molecular sieve, zeolite molecular sieve, and silicon titanium molecular sieve; and / or the organic oxygen-absorbing material includes at least one of phenolic antioxidants, amine antioxidants, and phosphite antioxidants.
[0145] Porous oxygen-absorbing materials include, but are not limited to, at least one of activated carbon, carbon molecular sieves, zeolite molecular sieves, and silicon-titanium molecular sieves. These materials are porous and can act as adsorbents to absorb both lattice oxygen and oxygen. It is understood that lattice oxygen released from the sodium supplement reaches the porous oxygen-absorbing material and is also adsorbed within its pores. Organic oxygen-absorbing materials include, but are not limited to, at least one of phenolic antioxidants, amine antioxidants, and phosphite antioxidants. These antioxidants react chemically with oxygen, oxidizing the antioxidant itself into products that have no adverse effects on the battery cell while consuming oxygen, thereby improving oxygen release.
[0146] In one embodiment, the phenolic antioxidant includes at least one of butylated hydroxyanisole, butylated hydroxytoluene, propyl gallate, and tert-butylhydroquinone; and / or the amine antioxidant includes at least one of naphthylamine, diphenylamine, and p-phenylenediamine; and / or the phosphite antioxidant includes at least one of bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, tris(2,4-di-tert-butylphenyl)phosphite, bis[2-methyl-4,6-bis(1,1'-dimethylethyl)phenol]ethyl phosphate, tetrakis(2,4-di-tert-butyloctaalkoxy-4,4-biphenyl)phosphate, (2,4,6-tri-tert-butylphenyl-2-butyl-2-ethyl)-1,3-propylene glycol phosphite, and di(2,4-di-p-isopropylphenyl)pentaerythritol diphosphite.
[0147] The phenolic antioxidants in this application include, but are not limited to, at least one of butylated hydroxyanisole, butylated hydroxytoluene, propyl gallate, and tert-butylhydroquinone. Amine antioxidants include, but are not limited to, at least one of naphthylamine, diphenylamine, and p-phenylenediamine. Phosphite antioxidants include, but are not limited to, at least one of bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, tris(2,4-di-tert-butylphenyl)phosphite, bis[2-methyl-4,6-bis(1,1-dimethylethyl)phenol]ethyl phosphate, tetrakis(2,4-di-tert-butyloctaalkoxy-4,4-biphenyl)phosphate, (2,4,6-tri-tert-butylphenyl-2-butyl-2-ethyl)-1,3-propylene glycol phosphite, and di(2,4-di-p-isopropylphenyl)pentaerythritol diphosphite.
[0148] In one embodiment, the Dv50 value of the sodium supplement material is in the range of greater than 1 μm and less than or equal to 30 μm, preferably 5 μm to 25 μm.
[0149] Dv50: Among the sample particles, 50% of the total volume of the particles have a particle size larger than this value, and another 50% of the total volume of the particles have a particle size smaller than this value; Dv50 can represent the median particle size of the sample.
[0150] Dv50 can be measured using methods known in the art. For example, GB / T 19077-2016 can be used to characterize the particle size using a Malvern laser particle size analyzer, such as a Malvern Mastersizer-3000.
[0151] Sodium-supplementing materials are used in the positive electrode coating to improve sodium loss during cycling. The sodium-supplementing materials need to be mixed with the positive electrode materials. The Dv50 of the sodium-supplementing materials within the above-mentioned range can improve the coating process, for example, improving gelation and improving the problem of uneven distribution of the sodium-supplementing materials. It is understandable that while maintaining the mass of the sodium-supplementing material, as the size of the sodium-supplementing material gradually increases, the number of particles of the sodium-supplementing material decreases, resulting in uneven distribution of the sodium-supplementing material in the active layer. When the size of the sodium-supplementing material is too small, the sodium-supplementing material is prone to agglomeration. This phenomenon results in a higher capacity in the coating area containing the sodium-supplementing material. During the sodium removal process, sodium may be precipitated at the negative electrode, placing higher demands on the capacity of the negative electrode. Therefore, setting the Dv50 of the sodium-supplementing material within the above-mentioned range can alleviate the above-mentioned problems.
[0152] Among the above-mentioned values greater than 1μm and less than or equal to 30μm, the values include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 1.01μm, 1.1μm, 2μm, 5μm, 7μm, 10μm, 12μm, 14μm, 16μm, 18μm, 20μm, 22μm, 25μm, 27μm, 29μm, 30μm, etc., as well as the range values between any two of the above-mentioned point values.
[0153] In the above-mentioned 5μm to 25μm, the values include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 5μm, 6μm, 8μm, 10μm, 112μm, 14μm, 15μm, 17μm, 19μm, 20μm, 22μm, 23μm, 24μm, 25μm, etc., as well as the range values between any two of the above-mentioned point values.
[0154] In one embodiment, the thickness of the coating layer ranges from 10 nm to 1000 nm, preferably, from 100 nm to 800 nm.
[0155] It is understandable that the thickness of the coating layer is within the above range, which can improve the escape of lattice oxygen and improve the release of oxygen. It is understandable that when the thickness of the coating layer is too low, it cannot play an effective physical isolation role and the oxygen adsorption amount is low. At the same time, when the coating layer is too thick, considering that the coating layer includes materials with poor conductivity, it may affect the conductive properties of the battery cell. Therefore, setting the thickness of the coating layer within the above range can improve the escape of sodium and improve the sodium replenishment effect.
[0156] In the above-mentioned 10nm to 1000nm, the values include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 10nm, 50nm, 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 950nm, 1000nm, etc., as well as the range values between any two of the above-mentioned point values.
[0157] In one embodiment, the thickness of the lattice oxygen stabilization layer is in the range of 10 nm to 400 nm, preferably 50 nm to 300 nm; and / or the thickness of the oxygen adsorption layer is in the range of 10 nm to 600 nm, preferably 50 nm to 500 nm.
[0158] When the thickness of the lattice oxygen stabilizing layer is within the above range, the release of lattice oxygen can be improved.
[0159] The thickness of the oxygen adsorption layer is within the above range, which can improve the adsorption and consumption of oxygen, thereby reducing the amount of oxygen entering the electrolyte.
[0160] In the above-mentioned 10nm to 400nm, the values include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 10nm, 50nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, etc., as well as the range values between any two of the above-mentioned point values.
[0161] In the above-mentioned 50nm to 300nm, the values include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 50nm, 100nm, 150nm, 200nm, 250nm, 300nm, etc., as well as the range values between any two of the above-mentioned point values.
[0162] In the above-mentioned 10nm to 600nm, the values include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 10nm, 50nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 500nm, 540nm, 580nm, 600nm, etc., as well as the range values between any two of the above-mentioned point values.
[0163] In the above-mentioned 50nm to 500nm, the values include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 50nm, 100nm, 130nm, 150nm, 180nm, 200nm, 220nm, 250nm, 270nm, 280nm, 290nm, 300nm, 340nm, 380nm, 400nm, 440nm, 480nm, 500nm, etc., as well as the range values between any two of the above-mentioned point values.
[0164] In one embodiment, the ratio of Dv50 of the sodium supplement to the Dv50 of the oxygen adsorbent is 5:1 to 250:1, and the oxygen adsorbent includes a porous oxygen-absorbing material; and / or, the Dv50 of the sodium supplement is in the range of 1 μm to 25 μm; and / or, the Dv50 of the oxygen adsorbent is in the range of 10 nm to 200 nm, and the oxygen adsorbent includes a porous oxygen-absorbing material.
[0165] Considering that when the porous oxygen-absorbing material is coated on the surface of the sodium supplementer, it is difficult to effectively coat the surface of the sodium supplementer if the particle size of the porous oxygen-absorbing material is too large, the ratio of the Dv50 of the sodium supplementer to the Dv50 of the oxygen adsorption material is set within the above range so that the porous oxygen-absorbing material can be effectively coated on the surface of the sodium supplementer.
[0166] The Dv50 of the sodium supplement agent is within the above range, which helps to obtain sodium supplement materials of appropriate size and facilitates the coating process operation after the sodium supplement material is mixed with the positive electrode material.
[0167] The Dv50 of the porous oxygen absorbing material is within the above range, so that the porous oxygen absorbing material can be effectively coated on the surface of the sodium supplement agent.
[0168] In the above 5:1 to 250:1, the values include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 5:1, 10:1, 50:1, 80:1, 100:1, 150:1, 200:1, 220:1, 250:1, etc., as well as the range values between any two of the above point values.
[0169] In the above-mentioned 1μm to 25μm, the values include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 1μm, 2μm, 5μm, 10μm, 15μm, 20μm, 25μm, etc., as well as the range values between any two of the above-mentioned point values.
[0170] In the above-mentioned 10nm to 200nm, the values include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 10nm, 20nm, 30nm, 50nm, 70nm, 90nm, 100nm, 120nm, 140nm, 160nm, 180nm, 190nm, 200nm, etc., as well as the range values between any two of the above-mentioned point values.
[0171] In one embodiment, the chemical formula of the sodium supplement includes Na x1 MO2 and / or Na x2 MO4, 2≤x1<4, 2≤x2<8, M includes at least one of Ni, Co, Mn, Al, Zr, Ti, V, Er, Ca, Fe, Ru, Ir, Sn, Cr, Cu, Nb, and Mo.
[0172] The chemical formula of the sodium supplement of the present application includes but is not limited to Na x1 MO2 and / or Na x2MO4, 2≤x1<4, 2≤x2<8, M includes at least one of Ni, Co, Mn, Al, Zr, Ti, V, Er, Ca, Fe, Ru, Ir, Sn, Cr, Cu, Nb, and Mo.
[0173] The sodium-supplementing material of the present application includes a sodium-supplementing agent and a coating layer provided on the surface of the sodium-supplementing agent, wherein the coating layer includes a lattice oxygen-stabilizing material and / or an oxygen-adsorbing material. The coating layer of the sodium-supplementing material of the present application includes three situations: one situation is that the coating layer includes a lattice oxygen-stabilizing material; another situation is that the coating layer includes an oxygen-adsorbing material; and another situation is that the coating layer includes a lattice oxygen-stabilizing material and an oxygen-adsorbing material.
[0174] In one embodiment, if Figure 3 As shown, the present application also provides a method for preparing a sodium supplement material, comprising: preparing a sodium supplement agent; mixing the sodium supplement agent with a lattice oxygen stabilizing material, and calcining to obtain a material, so that the lattice oxygen stabilizing material is coated on the surface of the sodium supplement agent; placing the above-mentioned calcined material and an oxygen adsorption material in a solvent and mixing them, and drying to obtain a sodium supplement material, so that the lattice oxygen stabilizing material and the oxygen adsorption material form a coating layer on the surface of the sodium supplement agent, the sodium supplement material comprises a sodium supplement agent and a coating layer provided on the surface of the sodium supplement agent, and the coating layer comprises the lattice oxygen stabilizing material and the oxygen adsorption material.
[0175] Alternatively, in one embodiment, a method for preparing a sodium-supplementing material includes: preparing a sodium-supplementing agent; mixing the sodium-supplementing agent with a lattice oxygen-stabilizing material, and calcining to obtain the sodium-supplementing material, so that the lattice oxygen-stabilizing material forms a coating layer on the surface of the sodium-supplementing agent, and the sodium-supplementing material obtained by calcination includes the sodium-supplementing agent and a coating layer provided on the surface of the sodium-supplementing agent, and the coating layer includes the lattice oxygen-stabilizing material; that is, the present application obtains a sodium-supplementing material having a sodium-supplementing agent coated with a lattice oxygen-stabilizing material by mixing the sodium-supplementing agent with the lattice oxygen-stabilizing material and calcining them.
[0176] Alternatively, in one embodiment, a method for preparing a sodium-supplementing material comprises: preparing a sodium-supplementing agent; mixing the sodium-supplementing agent and an oxygen adsorbing material in a solvent, and drying to obtain the sodium-supplementing material, so that the oxygen adsorbing material forms a coating layer on the surface of the sodium-supplementing agent, the sodium-supplementing material comprising the sodium-supplementing agent and a coating layer disposed on the surface of the sodium-supplementing agent, the coating layer comprising the oxygen adsorbing material; that is, the present application obtains a sodium-supplementing material comprising the oxygen adsorbing material coating the sodium-supplementing agent by mixing the sodium-supplementing agent and the oxygen adsorbing material in a solvent, and drying to obtain the sodium-supplementing material.
[0177] In one embodiment, the process of preparing the sodium supplementing agent includes the following steps: mixing a sodium source and a metal source, and calcining to obtain the sodium supplementing agent, wherein the calcination temperature is 500° C. to 1200° C., and the calcination time is 3 h to 12 h.
[0178] The sodium supplementer of the present application can be directly a commercial material or can be directly prepared from raw materials. During the preparation process, a sodium source and a metal source are mixed and calcined to obtain the sodium supplementer, wherein the calcination temperature is 500° C. to 1200° C. and the calcination time is 3 h to 12 h.
[0179] In the above-mentioned 500℃ to 1200℃, the values include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 500℃, 700℃, 800℃, 900℃, 1000℃, 1100℃, 1150℃, 1200℃, etc., as well as the range values between any two of the above-mentioned point values.
[0180] In the above 3h to 12h, the values include the minimum and maximum values of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, etc., as well as the range values between any two of the above point values.
[0181] In one embodiment, in the step of mixing the sodium supplement with the lattice oxygen stabilizing material and calcining to obtain the material, the lattice oxygen stabilizing material includes at least one of a transition metal oxide, a sulfide, and a phosphate, the calcination temperature is 200°C to 600°C, and the calcination time is 2h to 8h.
[0182] In the step of mixing the sodium supplement with the lattice oxygen stabilizing material and calcining to obtain the material, the lattice oxygen stabilizing material includes at least one of a transition metal oxide, a sulfide, and a phosphate, the calcination temperature is 200° C. to 600° C., and the calcination time is 2 h to 8 h.
[0183] In the above-mentioned 200℃ to 600℃, the values include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 200℃, 300℃, 400℃, 500℃, 600℃, etc., as well as the range values between any two of the above-mentioned point values.
[0184] In the above 2h to 8h, the values include the minimum and maximum values of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 2h, 3h, 4h, 5h, 6h, 7h, 8h, etc., as well as the range values between any two of the above point values.
[0185] In one embodiment, in the step of mixing the sodium supplement and the lattice oxygen stabilizing material and calcining to obtain the material, the lattice oxygen stabilizing material includes a conductive polymer, the calcination temperature is 150° C. to 450° C., and the calcination time is 2 h to 8 h.
[0186] The lattice oxygen-stabilized material includes a conductive polymer, and the calcination temperature is 150° C. to 450° C., and the calcination time is 2 hours to 8 hours.
[0187] In one embodiment, the sodium source includes at least one of sodium oxide, sodium hydroxide, sodium peroxide, sodium carbonate, sodium bicarbonate, sodium sulfate, sodium phosphate, sodium nitrate, sodium acetate, sodium chloride or sodium fluoride; and / or the mass ratio of the sodium supplement to the lattice oxygen stabilizing material ranges from 1% to 10%; and / or the mass ratio of the sodium supplement to the oxygen adsorbing material ranges from 1% to 10%; and / or the ratio of the Dv50 of the sodium supplement to the Dv50 of the oxygen adsorbing material is 5:1 to 250:1, and the oxygen adsorbing material includes a porous oxygen-absorbing material; and / or the solvent includes at least one of ethanol, ethylene glycol, diethylene glycol, and polyethylene glycol 400.
[0188] The sodium source of the present application includes but is not limited to at least one of sodium oxide, sodium hydroxide, sodium peroxide, sodium carbonate, sodium bicarbonate, sodium sulfate, sodium phosphate, sodium nitrate, sodium acetate, sodium chloride or sodium fluoride.
[0189] The mass ratio of the sodium supplement to the lattice oxygen stabilizing material is within the above range, and the thickness of the lattice oxygen stabilizing layer can be within a range of 10 nm to 400 nm.
[0190] The mass ratio of the sodium supplement to the oxygen adsorption material is within the above range, and the thickness of the oxygen adsorption layer can be in the range of 10 nm to 600 nm.
[0191] The ratio of the Dv50 of the sodium supplementer to the Dv50 of the porous oxygen absorbing material is within the above range, which can effectively coat the porous adsorption material on the surface of the sodium supplementer.
[0192] The solvent in the present application includes but is not limited to at least one of ethanol, ethylene glycol, diethylene glycol, and polyethylene glycol 400.
[0193] In one embodiment, the present application further provides a positive electrode plate, which includes the sodium-supplementing material as described above; or, the positive electrode plate includes the sodium-supplementing material obtained by the preparation method of the sodium-supplementing material as described above.
[0194] In one embodiment, the positive electrode plate includes an active material, and the mass of the sodium-supplementing material accounts for a percentage of the total mass of the active material and the sodium-supplementing material that is greater than 0 and less than or equal to 20%, preferably, 5% to 15%.
[0195] The loss of sodium ions leads to very low first-cycle efficiency in sodium-ion batteries, ranging from approximately 50% to 85%. Adjusting the mass percentage of the sodium-supplementing material to the total mass of the active material and the sodium-supplementing material within this range can compensate for this loss and improve battery performance. It is understood that if the mass percentage of the sodium-supplementing material to the total mass of the active material and the sodium-supplementing material is too large, the amount of active material used will be reduced. Given that the performance of the sodium-supplementing material is inferior to that of the active material, increasing the amount of the sodium-supplementing material in this situation will reduce battery performance.
[0196] In one embodiment, the present application further provides an electrode assembly, which includes a negative electrode plate, an electrolyte, and the positive electrode plate as described above.
[0197] Since the positive electrode plate adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.
[0198] In one embodiment, the present application also provides a battery, which includes the electrode assembly as described above.
[0199] Since the electrode assembly adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.
[0200] It is understandable that batteries include battery cells, battery modules, and battery packs.
[0201] In one embodiment, the present application further provides an electrical device, which includes the battery as described above.
[0202] Since the battery adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.
[0203] In addition, the battery (battery cell, battery module, battery pack) and the electric device of the present application will be described below with reference to the drawings as appropriate.
[0204] In one embodiment of the present application, a battery cell is provided.
[0205] Typically, a battery cell consists of a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery's charge and discharge processes, active ions are embedded in and extracted from the positive and negative electrodes. The electrolyte conducts ions between the positive and negative electrodes. The separator, located between the positive and negative electrodes, primarily prevents short circuits between the positive and negative electrodes while allowing ions to pass through. The separator is the separator described above in this application.
[0206] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector.
[0207] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.
[0208] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy) on a polymer substrate (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0209] In some embodiments, the positive electrode film layer may further optionally include a binder. For example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.
[0210] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0211] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0212] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0213] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0214] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy) on a polymer substrate (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0215] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and the like. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0216] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0217] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0218] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0219] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0220] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. This application has no specific restrictions on the type of electrolyte, and it can be selected according to needs.
[0221] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.
[0222] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0223] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0224] In some embodiments, the battery cell further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0225] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0226] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.
[0227] In some embodiments, the battery cell may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0228] In some embodiments, the outer packaging of the battery cell may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the battery cell may be a soft shell, such as a pouch-type soft shell. The soft shell may be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0229] The present application has no particular restrictions on the shape of the battery cell, which can be cylindrical, square or any other shape. For example, Figure 4 The battery cell 5 is a square structure as an example.
[0230] In some embodiments, reference Figure 5The outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the diaphragm can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is impregnated in the electrode assembly 52. The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0231] In some embodiments, battery cells may be assembled into a battery module. The battery module may contain one or more battery cells. The specific number may be selected by those skilled in the art based on the application and capacity of the battery module.
[0232] Figure 6 4 is an example of a battery module. Figure 6 In the battery module 4, the plurality of battery cells 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. The plurality of battery cells 5 may further be fixed by fasteners.
[0233] Optionally, the battery module 4 may further include a housing having an accommodation space, and the plurality of battery cells 5 are accommodated in the accommodation space.
[0234] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.
[0235] Figure 7 and Figure 8 The battery pack 1 is used as an example. Figure 7 and Figure 8 The battery pack 1 may include a battery box and multiple battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner in the battery box.
[0236] In addition, the present application also provides an electrical device, which includes at least one of the battery cells, battery modules, or battery packs provided in the present application. The battery cells, battery modules, or battery packs can serve as power sources for the electrical device or as energy storage units for the electrical device. Electrical devices may include, but are not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships, satellites, energy storage systems, etc.
[0237] As an electrical device, a battery cell, battery module or battery pack can be selected according to its usage requirements.
[0238] Figure 9 This is an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the battery cells in this device, a battery pack or battery module can be used.
[0239] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be lightweight and thin, and may use a battery cell as a power source.
[0240] Example
[0241] Example 1
[0242] Preparation of sodium supplement materials
[0243] The sodium source (sodium carbonate) and the transition metal source (Ni(OH)2) are uniformly mixed in a molar ratio of 1.05:1, compacted into blocks, and calcined to obtain a sodium supplement; the calcination temperature is 800°C and the calcination time is 8 hours.
[0244] The sodium supplement agent and the lattice oxygen stabilizing material (V2O5) are calcined in a mass ratio of 3:97 to obtain a material so that the lattice oxygen stabilizing material is coated on the surface of the sodium supplement agent; the calcination temperature is 400°C and the calcination time is 6 hours.
[0245] The calcined material and an oxygen adsorption material (activated carbon, the Dv50 of the activated carbon is 10 nm) are placed in ethanol and mixed, and dried to obtain a sodium supplementing material, so that the lattice oxygen stabilizing material and the oxygen adsorption material form a coating layer on the surface of the sodium supplementing agent. The sodium supplementing material includes a sodium supplementing agent and a coating layer provided on the surface of the sodium supplementing agent, the coating layer includes the lattice oxygen stabilizing material and the oxygen adsorption material, and the mass ratio of the sodium supplementing agent to the oxygen adsorption material is 5:95.
[0246] The chemical formula of the sodium supplement is Na2NiO2 (the Dv50 value of the sodium supplement is 1260nm), the Dv50 value of the sodium supplement material is (15μm), the thickness of the lattice oxygen stabilization layer is (200nm), and the thickness of the oxygen adsorption layer is (40nm).
[0247] Preparation of sodium positive electrode
[0248] Prepare sodium positive electrode active material (NaFePO4) and the above-mentioned sodium supplement material, binder (PVDF), and conductive agent (acetylene black), and mix them in a mass ratio of 90:5:5, wherein the mass of the above-mentioned sodium supplement material accounts for 5% of the total mass of the positive electrode active material and the sodium supplement material, and add a solvent (N-methylpyrrolidone) to prepare a slurry, apply the slurry on and then evenly coat the slurry on the aluminum foil current collector, and then dry, cold press, and cut to obtain the positive electrode sheet.
[0249] Preparation of negative electrode sheet
[0250] The active material artificial graphite, the conductive agent carbon black, the binder styrene-butadiene rubber (SBR), and the thickener sodium carboxymethyl cellulose (CMC) are dissolved in the solvent deionized water in a weight ratio of 96.2:0.8:0.8:1.2, and mixed evenly to prepare the negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode current collector copper foil once or multiple times, and the negative electrode sheet is obtained after drying, cold pressing, and slitting.
[0251] Preparation of electrolyte
[0252] In an argon atmosphere glove box (H2O <0.1ppm, O2 <0.1ppm), the organic solvents ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 3 / 7, 12.5% NaPF6 sodium salt was added and dissolved in the organic solvent, and stirred evenly.
[0253] Isolation film
[0254] Polypropylene film is used as the isolation film.
[0255] Preparation of sodium ion batteries
[0256] The positive electrode sheet, separator, and negative electrode sheet of Example 1 were stacked in order, with the separator positioned between the positive and negative electrode sheets to provide isolation. The cells were then wound to obtain a bare cell. The tabs were welded to the bare cell and placed in an aluminum shell. The cells were then baked at 100°C to remove water, and then electrolyte was injected and sealed to obtain an uncharged battery. The uncharged battery then underwent a series of steps, including resting, hot and cold pressing, formation, shaping, and capacity testing, to obtain the sodium-ion battery product of Example 1.
[0257] Example 2
[0258] On the basis of Example 1, the ratio of the mass of the sodium-supplementing material to the total mass of the positive electrode active material and the sodium-supplementing material was adjusted to 10%.
[0259] Example 3
[0260] On the basis of Example 1, the ratio of the mass of the sodium-supplementing material to the total mass of the positive electrode active material and the sodium-supplementing material was adjusted to 15%.
[0261] Example 4 to Example 6
[0262] On the basis of Example 2, the type of lattice oxygen stabilizing material is adjusted.
[0263] Example 7 and Example 8
[0264] On the basis of Example 2, the type of oxygen adsorbent was adjusted.
[0265] Example 9 and Example 12
[0266] Based on Example 2, the particle size of the sodium supplementing material was adjusted.
[0267] Example 13 and Example 16
[0268] Based on Example 2, the thickness of the lattice oxygen stabilization layer is adjusted.
[0269] Example 17 and Example 20
[0270] Based on Example 2, the thickness of the oxygen adsorption layer was adjusted.
[0271] Example 21
[0272] On the basis of Example 2, the lattice oxygen stabilizing material is adjusted to include V2O5 and titanium disulfide, and the mass ratio of the two is 50:50.
[0273] Example 22
[0274] On the basis of Example 2, the oxygen adsorption material is adjusted to include activated carbon and butylated hydroxyanisole, and the mass ratio of the two is 50:50.
[0275] Example 23
[0276] On the basis of Example 2, only the lattice oxygen stabilization layer is included.
[0277] Preparation of sodium supplement materials
[0278] The sodium source (sodium carbonate) and the transition metal source (Ni(OH)2) are uniformly mixed in a molar ratio of 1.05:1, compacted into blocks, and calcined to obtain a sodium supplement; the calcination temperature is 800°C and the calcination time is 8 hours.
[0279] A sodium supplementing agent and a lattice oxygen stabilizing material (V2O5) are calcined in a mass ratio of 3:97 to obtain a sodium supplementing material, so that the lattice oxygen stabilizing material forms a coating layer on the surface of the sodium supplementing agent. The sodium supplementing material obtained by calcination includes the sodium supplementing agent and a coating layer arranged on the surface of the sodium supplementing agent, and the coating layer includes the lattice oxygen stabilizing material; the calcination temperature is 400°C and the calcination time is 6 hours.
[0280] The chemical formula of the sodium supplement agent is Na2NiO2, the Dv50 value of the sodium supplement material is (15μm), and the thickness of the lattice oxygen stabilization layer is (200nm).
[0281] Example 24
[0282] On the basis of Example 2, only the oxygen adsorption layer is included.
[0283] Preparation of sodium supplement materials
[0284] The sodium source (sodium carbonate) and the transition metal source (Ni(OH)2) are uniformly mixed in a molar ratio of 1.05:1, compacted into blocks, and calcined to obtain a sodium supplement; the calcination temperature is 800°C and the calcination time is 8 hours.
[0285] A sodium supplementing agent and an oxygen adsorption material (activated carbon, the Dv50 of the activated carbon is 10 nm) are placed in ethanol and mixed, and the sodium supplementing material is obtained after drying, so that the oxygen adsorption material forms a coating layer on the surface of the sodium supplementing agent. The sodium supplementing material includes the sodium supplementing agent and a coating layer provided on the surface of the sodium supplementing agent, the coating layer includes the oxygen adsorption material, and the mass ratio of the sodium supplementing agent to the oxygen adsorption material is 5:95.
[0286] The chemical formula of the sodium supplement is Na2NiO2, the Dv50 value of the sodium supplement material is (15 μm), and the thickness of the oxygen adsorption layer is (40 nm).
[0287] Comparative Example 1
[0288] On the basis of Example 1, no sodium supplement material was added.
[0289] Full battery first performance test steps
[0290] After filling, the battery cell undergoes two charging and discharging processes: formation and capacity separation. The first step of both formation and capacity separation involves charging, and the sum of these two capacities is the initial charge capacity of the full battery. The second step of the capacity separation process involves discharging from a fully charged state to an empty state, so the capacity at this step is the discharge capacity of the full battery. Combining these two steps yields the formula for calculating the initial efficiency of the full battery: initial efficiency of the full battery = discharge capacity in the second capacity separation step / (charge capacity in formation + charge capacity in the first capacity separation step).
[0291] Full battery capacity test steps
[0292] At 25°C, the battery cell is first charged to 4.3V at a constant current of 1C, further charged at a constant voltage of 4.3V to a current of 0.05C, and then discharged to 2V at a constant current of 1C. The discharge capacity at this time is recorded as the cell capacity.
[0293] Cyclic performance test steps
[0294] At 45°C, the battery cell is first charged to 4.3V at a constant current of 1C, then further charged at a constant voltage of 4.3V to a current of 0.05C, and then discharged to 2V at a constant current of 1C. This is a charge and discharge cycle process, and the discharge capacity this time is the discharge capacity of the first cycle. The battery is subjected to multiple cycle charge and discharge tests in the above manner, and the discharge capacity of the 200th cycle is detected. The capacity retention rate of the battery cell after the cycle is calculated using the following formula. The capacity retention rate of the battery after 200 cycles (wt%) = [discharge capacity of the 200th cycle / discharge capacity of the first cycle] × 100wt%.
[0295] Table 1 Experimental data list
[0296]
[0297] As can be seen from the table above, the present application improves battery performance by adding a sodium-supplementing material to the positive electrode. Furthermore, a comparison of Example 2, Example 23, and Example 24 shows that when the sodium-supplementing material includes both a lattice oxygen-stabilizing material and an oxygen-absorbing material, the battery's cycling performance is even better. This indicates that the lattice oxygen-stabilizing material can stabilize the structure of the sodium-supplementing agent, improve the release of lattice oxygen, and reduce the amount of oxygen released. The oxygen-absorbing layer can filter the released oxygen and reduce the amount of oxygen entering the electrolyte. The lattice oxygen-stabilizing material and the oxygen-absorbing material can improve the release of oxygen from the sodium-supplementing material and thus improve battery performance.
[0298] The above are only preferred embodiments of the present invention and are not intended to limit the patent scope of the present invention. All equivalent structural transformations made using the contents of the present invention's description and drawings under the inventive concept of the present invention, or direct / indirect applications in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A sodium supplement material, It is characterized in that The sodium supplement material comprises a sodium supplement agent and a coating layer arranged on the surface of the sodium supplement agent. The coating layer includes a lattice oxygen stabilizing material and / or an oxygen absorbing material; The chemical formula of the sodium supplement includes Na x1 MO 2 and / or Na x2 MO 4 , 2≤x1<4, 2≤x2<8, M includes at least one of Ni, Co, Mn, Al, Zr, Ti, V, Er, Ca, Fe, Ru, Ir, Sn, Cr, Cu, Nb, and Mo; The coating layer includes a lattice oxygen stabilization layer and an oxygen adsorption layer, wherein the lattice oxygen stabilization layer is disposed on the surface of the sodium supplement, and the oxygen adsorption layer is disposed on the surface of the lattice oxygen stabilization layer; The lattice oxygen stabilizing layer comprises a lattice oxygen stabilizing material, and the oxygen adsorption layer comprises an oxygen adsorption material; The lattice oxygen stabilizing material comprises a composite of a transition metal oxide and at least one of a sulfide, a phosphate, and a conductive polymer, and the lattice oxygen stabilizing material forms a physical barrier layer on the surface of the sodium supplement; The oxygen absorbing material includes a porous oxygen absorbing material.
2. The sodium supplement material according to claim 1, It is characterized in that The lattice oxygen stabilization layer completely covers the surface of the sodium supplement; And / or, the oxygen adsorption layer completely covers the surface of the lattice oxygen stabilization layer.
3. The sodium supplement material according to claim 1, It is characterized in that The transition metal oxide includes V 2 O 5 、ZrO 2 、TiO 2 、RuO 2 ,La 2 O 3 、CeO 2 At least one of; And / or, the sulfide includes at least one of titanium disulfide, iron sulfide, cobalt sulfide, nickel sulfide, molybdenum sulfide, tin sulfide, and antimony sulfide; And / or, the phosphate includes at least one of titanium phosphate, titanium pyrophosphate, sodium titanium phosphate, sodium aluminum titanium phosphate, and sodium vanadium phosphate; And / or, the conductive polymer includes at least one of polypyrrole, polyethylene glycol, polyaniline, and poly(3,4-ethylenedioxythiophene).
4. The sodium supplement material according to claim 1, It is characterized in that The porous oxygen absorbing material comprises at least one of activated carbon, carbon molecular sieve, zeolite molecular sieve and silicon titanium molecular sieve; And / or, the oxygen absorbing material further includes an organic oxygen absorbing material, and the organic oxygen absorbing material includes at least one of a phenolic antioxidant, an amine antioxidant, and a phosphite antioxidant.
5. The sodium supplement material according to claim 4, It is characterized in that The phenolic antioxidant includes at least one of butylated hydroxyanisole, butylated hydroxytoluene, propyl gallate and tert-butylhydroquinone; And / or, the amine antioxidant includes at least one of naphthylamine, diphenylamine, and p-phenylenediamine; And / or, the phosphite antioxidant includes at least one of bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, tris(2,4-di-tert-butylphenyl)phosphite, bis[2-methyl-4,6-di(1,1-dimethylethyl)phenol]ethyl phosphate, tetrakis(2,4-di-tert-butyloctaalkoxy-4,4-biphenyl)phosphate, (2,4,6-tri-tert-butylphenyl-2-butyl-2-ethyl)-1,3-propylene glycol phosphite, and di(2,4-di-p-isopropylphenyl)pentaerythritol diphosphite.
6. The sodium supplement material according to any one of claims 1 to 5, It is characterized in that The Dv50 range value of the sodium supplement material is greater than 1 μm and less than or equal to 30 μm.
7. The sodium supplement material according to claim 6, It is characterized in that The Dv50 value of the sodium supplement material ranges from 5 μm to 25 μm.
8. The sodium supplement material according to any one of claims 1 to 5 and 7, It is characterized in that The thickness of the coating layer ranges from 10 nm to 1000 nm.
9. The sodium supplement material according to claim 8, It is characterized in that The thickness of the coating layer ranges from 100 nm to 800 nm.
10. The sodium supplement material according to claim 1 or 2, It is characterized in that The thickness of the lattice oxygen stabilization layer ranges from 10 nm to 400 nm; And / or, the thickness of the oxygen adsorption layer ranges from 10 nm to 600 nm.
11. The sodium supplement material according to claim 10, It is characterized in that The thickness of the lattice oxygen stabilization layer ranges from 50 nm to 300 nm; And / or, the thickness of the oxygen adsorption layer ranges from 50 nm to 500 nm.
12. The sodium supplement material according to any one of claims 1 to 5, 7, 9, and 11, It is characterized in that The ratio of the Dv50 of the sodium supplement to the Dv50 of the oxygen adsorbent material is 5:1 to 250:1, and the oxygen adsorbent material comprises a porous oxygen absorbing material; And / or, the Dv50 value of the sodium supplement is in the range of 1 μm to 25 μm; And / or, the Dv50 value of the oxygen adsorbing material is in the range of 10 nm to 200 nm, and the oxygen adsorbing material comprises a porous oxygen absorbing material.
13. A method for preparing the sodium supplement material according to any one of claims 1 to 12, It is characterized in that include: Prepare sodium supplements; The sodium supplementing agent is mixed with a lattice oxygen stabilizing material, and calcined to obtain the sodium supplementing material, so that the lattice oxygen stabilizing material forms a coating layer on the surface of the sodium supplementing agent, wherein the sodium supplementing material obtained by calcination comprises the sodium supplementing agent and the coating layer disposed on the surface of the sodium supplementing agent, and the coating layer comprises the lattice oxygen stabilizing material; Alternatively, the method for preparing the sodium supplement material comprises: Prepare sodium supplements; The sodium supplementing agent and the oxygen adsorbing material are placed in a solvent and mixed, and dried to obtain the sodium supplementing material, so that the oxygen adsorbing material forms a coating layer on the surface of the sodium supplementing agent, the sodium supplementing material comprises the sodium supplementing agent and the coating layer arranged on the surface of the sodium supplementing agent, and the coating layer comprises the oxygen adsorbing material; Alternatively, the method for preparing the sodium supplement material comprises: Prepare sodium supplements; The sodium supplement agent is mixed with a lattice oxygen stabilizing material, and calcined to obtain a material, so that the lattice oxygen stabilizing material is coated on the surface of the sodium supplement agent; The calcined material is placed in a solvent and mixed with an oxygen adsorbing material, and then dried to obtain a sodium supplementing material, so that the lattice oxygen stabilizing material and the oxygen adsorbing material form a coating layer on the surface of the sodium supplementing agent. The sodium supplementing material includes a sodium supplementing agent and the coating layer arranged on the surface of the sodium supplementing agent, and the coating layer includes the lattice oxygen stabilizing material and the oxygen adsorbing material.
14. The method for preparing the sodium supplement material according to claim 13, It is characterized in that In preparing the sodium supplement, the following steps are included: A sodium source and a metal source are mixed and calcined to obtain a sodium supplement agent, wherein the calcination temperature is 500° C. to 1200° C. and the calcination time is 3 h to 12 h.
15. The method for preparing the sodium supplement material according to claim 13 or 14, It is characterized in that In the step of mixing the sodium supplement with a lattice oxygen-stabilizing material and calcining to obtain the material, the lattice oxygen-stabilizing material includes at least one of a transition metal oxide, a sulfide, and a phosphate, the calcination temperature is 200° C. to 600° C., and the calcination time is 2 h to 8 h.
16. The method for preparing the sodium supplement material according to claim 13 or 14, It is characterized in that In the step of mixing the sodium supplement with the lattice oxygen-stabilized material and calcining to obtain the material, the lattice oxygen-stabilized material includes a conductive polymer, the calcination temperature is 150° C. to 450° C., and the calcination time is 2 h to 8 h.
17. The method for preparing the sodium supplement material according to claim 14, It is characterized in that The sodium source includes at least one of sodium oxide, sodium hydroxide, sodium peroxide, sodium carbonate, sodium bicarbonate, sodium sulfate, sodium phosphate, sodium nitrate, sodium acetate, sodium chloride or sodium fluoride; and / or, the mass ratio of the sodium supplement to the lattice oxygen stabilizing material is in a range of 1% to 10%; And / or, the mass ratio of the sodium supplement to the oxygen adsorbent is in the range of 1% to 10%; and / or, the ratio of the Dv50 of the sodium supplement to the Dv50 of the oxygen adsorbent is 5:1 to 250:1, and the oxygen adsorbent comprises a porous oxygen absorbing material; And / or, the solvent includes at least one of ethanol, ethylene glycol, diethylene glycol, and polyethylene glycol 400.
18. A positive electrode sheet, It is characterized in that The positive electrode plate comprises a sodium supplement material as claimed in any one of claims 1 to 12; Alternatively, the positive electrode plate includes a sodium-supplementing material obtained by the method for preparing a sodium-supplementing material according to any one of claims 13 to 17.
19. The positive electrode sheet according to claim 18, It is characterized in that The positive electrode plate includes an active material, and the mass of the sodium supplement material accounts for a percentage of the total mass of the active material and the sodium supplement material that is greater than 0 and less than or equal to 20%.
20. The positive electrode sheet according to claim 19, It is characterized in that The mass of the sodium supplementing material accounts for 5% to 15% of the total mass of the active material and the sodium supplementing material.
21. An electrode assembly, It is characterized in that The electrode assembly comprises a negative electrode sheet, an electrolyte and a positive electrode sheet as claimed in any one of claims 18 to 20.
22. A battery, It is characterized in that The battery comprises the electrode assembly of claim 21.
23. An electrical device, It is characterized in that The electrical device comprises the battery as claimed in claim 22.