A pipeline outer wall surfacing process
Through the outer wall surfacing process, CNC equipment and appropriate welding wire inclination angle are used to form a uniform columnar crystal distribution, which solves the problem of low creep resistance of the pressure furnace pipeline, extends the service life and improves economic benefits.
Patent Information
- Application Number
- CN202310383850.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-12
AI Technical Summary
The creep resistance of pressure furnace tube pipes is low, resulting in a short service life of the equipment under high temperature, high pressure and corrosive media.
The outer wall surfacing process is adopted, and the rotation and translation of the pipe are controlled by CNC equipment. The inclination angle between the welding wire and the pipe surface is 60° to 80°, forming a uniform distribution of columnar crystals. Multi-layer surfacing is performed and post-heat treatment and polishing are performed to ensure welding. quality and mechanical properties.
The creep resistance of the pipeline is improved, the service life is extended, and the economic benefits are significantly improved.
Smart Images

Figure CN116652456B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cladding, and in particular relates to a pipeline outer wall cladding process. Background Art
[0002] In the fields of petrochemical, nuclear power, metallurgy, etc., there are a large number of pressure pipeline equipment serving under high temperature and high pressure, corrosive media or cyclic loads. In recent years, my country's thermal power and chemical industries have developed rapidly, and production capacity and related production technologies have been greatly improved. Correspondingly, various types of pressure-bearing equipment have also developed towards large-scale and high-parameters with the advancement of industrial technology. Among them, pressure pipelines are key components of various pressure-bearing equipment. They are not only transportation channels for raw materials and products, but also places where some reactions occur. Their importance is self-evident. With the development of equipment and technology, pressure furnace pipes need to be continuously improved and upgraded as the operating temperature increases. At the same time, due to the complexity of its working environment, high requirements are placed on the selection of pipeline materials. The pipeline itself needs to have good mechanical properties to ensure the safe and effective operation of the equipment.
[0003] At present, judging the creep resistance of materials by microstructure has been widely used in the field of materials. One of them is the crystal boundary load-bearing theory, which uses the arrangement law of microscopic grains in the direction perpendicular to the force of the material as a reference, and can well correlate metal creep damage with microstructure. By analyzing the microstructure of the same weld creep specimen in three different force directions, two different causes of creep damage can be obtained. The first is that there are many three-crystal intersections at the grain boundaries in the direction perpendicular to the force, which can easily lead to stress concentration and creep holes are easy to initiate. With the further evolution of the damage, wedge-shaped cracks will appear at the grain boundaries / subgrain boundaries parallel to the force direction, further reducing the bearing area of the specimen. There are obvious subgrain boundaries inside the crystal in the direction perpendicular to the force, and creep holes will also appear here, so the creep holes will be locally concentrated (see Figure 1 (a)). The second type is that the grain boundary perpendicular to the force direction is long, so there are relatively few three-grain intersection points. Although the applied load is the same as the second case, the specific stress acting on the local grain boundary is relatively small, so it is mainly creep holes grown under diffusion (see Figure 1 (b)). Figure 1 (c) is the fracture life of the same material under two microscopic stress conditions under different stresses. Compared with the first microstructure condition, the actual life of the material under the second microstructure and stress distribution is longer.
[0004] Although the above theory has been applied to explain the creep damage of metal materials, it has not been actually applied to the current stage of strengthening the creep resistance of pressure furnace pipes. Therefore, the present invention designs a surfacing process based on the theory to improve the creep resistance of pressure furnace pipes. Summary of the invention
[0005] The purpose of the present invention is to provide a pipeline outer wall cladding process to effectively solve the problem of low creep resistance of pressure furnace pipes.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0007] A pipeline outer wall cladding process comprises the following steps:
[0008] S1. Derust, dehumidify, degrease and perform non-destructive testing on the welding area of the outer wall of the pipeline, and select the model and specification of the welding wire and the protective gas during welding according to the actual working environment and the thickness of the single-layer cladding;
[0009] S2. Adopt the form of outer wall cladding. After the pipeline is preheated, the welding is performed by keeping the welding gun in the same position and manipulating the pipeline to rotate continuously and move axially. During the welding process, the pipeline is regulated by the numerical control equipment to rotate and translate smoothly and at a steady speed. The welding equipment performs cladding at a fixed position. The specific rotation speed of the pipeline is determined according to the appropriate welding speed for cladding. The inclination angle between the welding wire and the pipeline surface is 60° to 80°, so as to realize the regulation of the internal structure of the cladding layer of the pipeline;
[0010] S3. When multiple layers of cladding are required, except for the last layer, the cladding surface needs to be post-heat treated after each layer of cladding and then polished to remove slag and spatter;
[0011] S4. After the surfacing is completed, heat treatment is carried out and non-destructive testing is passed, and the surfacing process is completed.
[0012] Furthermore, in step S2, the welding direction is from one end of the pipe to the other end along a spiral trajectory.
[0013] Furthermore, when there is a requirement for the thickness of the pipeline, multi-layer cladding should be performed to meet the thickness requirement.
[0014] Furthermore, the inclination angle between the welding wire and the pipeline surface in step S2 is determined according to the surfacing material and the welding environment.
[0015] Furthermore, the microscopic crystals of the surfacing layer of the pipe are columnar crystals, the direction of the columnar crystals is the same as the direction of the welding wire, and the arrangement of the columnar crystals is uniformly distributed in the surfacing layer.
[0016] The beneficial technical effects of the present invention are:
[0017] The surfacing process provided by the present invention enables the columnar crystal distribution of the pipeline surfacing layer to have an obvious uniform distribution rule along the wall thickness, thereby making the stress conditions of the pipeline more reasonable when subjected to circumferential and axial loads, improving the creep resistance of the pipeline, thereby extending the service life of the pipeline and greatly improving the economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.
[0019] Figure 1 It is a schematic diagram of the effect of inhomogeneous structure on creep damage;
[0020] Figure 2 This is the metallographic image of the VDF cracking furnace pipe sample before cladding;
[0021] Figure 3 It is the columnar crystal arrangement law of VDF cracking furnace pipeline before cladding;
[0022] Figure 4 It is the stress condition of microscopic columnar crystals of VDF cracking furnace pipeline before cladding under axial and hoop stress;
[0023] Figure 5 It is the microscopic stress condition of the ideal arrangement of columnar crystals under axial and hoop stress;
[0024] Figure 6 It is a schematic diagram of a specific embodiment of the present invention;
[0025] Figure 7 It is the metallographic diagram of the VDF cracking furnace pipeline sample after cladding and the corresponding microscopic crystal arrangement. DETAILED DESCRIPTION
[0026] The present invention adopts the crystal boundary bearing theory to explore the microscopic crystal arrangement of the pipeline without additional processing technology, summarizes the mechanical performance defects caused by its microscopic crystal arrangement, and derives the crystal arrangement under ideal conditions according to the specific stress conditions under the actual working conditions of the pipeline. With the best microscopic crystal arrangement as the goal, the best process scheme is determined to be the processing technology of external wall surfacing, and the control method of its microscopic crystal arrangement and the implementation process of the process are determined.
[0027] Below, the VDF cracking furnace tube is taken as a representative of the pressure furnace tube, the microstructure of the VDF cracking furnace tube is analyzed and its optimal microstructure form is obtained.
[0028] Figure 2 This is the metallographic diagram of the VDF cracking furnace pipe sample before cladding. Figure 2 (a) shows the metallographic image of the annular section of the pipeline in zone A. Figure 2(b) shows the metallographic image of the longitudinal section of the pipe in zone B. Figure 2 (c) shows an enlarged view of the outer layer of the pipe in zone C. Figure 2 (d) shows an enlarged view of the inner wall of the pipe in zone D.
[0029] Figure 3 This is the columnar crystal arrangement pattern of the VDF cracking furnace pipeline before cladding. Figure 3 (a) shows the crystal arrangement of section A. Figure 3 (b) shows the crystal arrangement of the B section. Figure 3 (c) shows the columnar crystal arrangement.
[0030] The raw material of the VDF cracking furnace tube is N6 pure nickel. Figure 2 As shown, the VDF cracking furnace pipeline is sampled and the microstructure morphology of each cross section is obtained, so as to analyze the microstructure of each cross section and obtain the internal crystal arrangement. Figure 3 As shown, the distribution direction of the microscopic columnar crystals of the VDF cracking furnace pipeline is along the axial direction of the pipeline.
[0031] The stress state of microscopic columnar crystals in the VDF cracking furnace pipeline under different stresses is analyzed, mainly focusing on the stress state of microscopic grain boundaries under the conditions of pipeline annular force and axial force with larger loads in actual working conditions. Figure 4 (a) shows the stress of microscopic columnar crystals under axial stress, such as Figure 4 As shown in (a), in the vertical force direction of the VDF cracking furnace pipeline under the action of axial force, there are many columnar crystal three-crystal intersection nodes. The crystal intersection nodes are the main stress-bearing sites, which are prone to stress concentration and damage, resulting in the initiation of creep holes. With the further evolution of the damage, wedge-shaped cracks will appear at the grain boundaries / subgrain boundaries parallel to the force direction. Figure 4 (b) shows the stress condition of microscopic columnar crystals under hoop stress, such as Figure 4 As shown in (b), the grain boundaries of the VDF cracking furnace pipeline in the vertical force direction under the action of the circumferential force are longer, the three-grain intersection points are relatively small, and part of the stress is shared to a certain extent at the grain boundaries. Therefore, under the same external load, the local stress is smaller, and the long grain boundaries will limit the expansion of creep holes at the grain boundaries. However, due to the presence of more non-columnar crystals in its microstructure composition, the length of the grain boundaries in the vertical force direction is not uniform, and local stress concentration is still prone to occur, so there is room for improvement.
[0032] By analyzing the actual stress conditions of the VDF cracking furnace pipeline, it can be concluded that the best microstructure of the pressure pipeline is a microstructure consisting entirely of columnar crystals distributed along the wall thickness direction, such as Figure 5This microstructure can maintain the stress state of the grain boundary of the pipeline material in a uniform distribution along the long grain boundary at the hoop stress and axial stress with large loads, making its stress distribution more uniform, thereby reducing stress concentration. This optimal microstructure can be applied to the creep resistance analysis of pipelines in various fields.
[0033] After studying and analyzing the wire welding process, the applicant has concluded that the microstructure pattern produced during wire cladding is that each wire weld will form a columnar crystal microstructure in the same direction as the wire, and its microstructure is completely composed of columnar crystals. For pressure pipes with relatively small inner diameters, the use of outer wall cladding can reinforce the original pipe while ensuring that the material flow of the original pipe inner wall is not affected by the thickness of the cladding, and the difficulty of implementing outer wall cladding in controlling the microstructure arrangement pattern is significantly lower than that of inner wall cladding.
[0034] Therefore, taking the microstructure morphology composed entirely of columnar crystals distributed along the wall thickness direction as the goal of the pipeline processing technology, and based on the microstructure laws produced during the wire cladding process, the applicant has developed a pipeline outer wall cladding process that is different from the traditional pipeline inner wall cladding process, thereby obtaining a microstructure arrangement form with better mechanical properties.
[0035] The present invention provides a pipeline outer wall cladding process, comprising the following steps:
[0036] S1. The welding area of the outer wall of the pipeline is derusted, dehumidified, degreased and non-destructively tested, and the model and specification of the welding wire and the protective gas during welding are selected according to the actual working environment and the thickness of the single-layer cladding.
[0037] S2, adopt the form of external wall cladding, after the pipeline is preheated, such as Figure 6 As shown, welding is performed by keeping the welding gun in a constant position and manipulating the pipe to rotate continuously and move axially. The welding direction is from one end of the pipe to the other end along a spiral trajectory. During the welding process, the pipe is controlled by a numerical control device to rotate and translate at a steady speed. The welding equipment performs surfacing welding at a fixed position. The specific rotation speed of the pipe is determined according to the appropriate welding speed for surfacing welding.
[0038] During the welding process, the angle between the welding wire and the surface of the welding pipe needs to ensure both the microstructure arrangement and the specific implementation process. In the welding process of the laboratory test, if the optimal microscopic columnar crystal arrangement is considered alone and the angle between the welding wire and the surface of the welding pipe is unilaterally set to 80°~90°, the welding wire metal will not be completely solidified during the welding process and will flow and drip during the rotation of the pipe, resulting in poor final welding quality; and if the angle between the welding wire and the surface of the welding pipe is too low, its microscopic columnar crystal arrangement will not meet the requirements of mechanical property strengthening. Therefore, the applicant has determined through a large number of experiments that the inclination angle between the welding wire and the pipe surface should be selected between 60° and 80° according to the surfacing material and the welding environment, so as to achieve the regulation of the internal structure of the surfacing layer of the pipe.
[0039] S3. When there is a requirement for the thickness of the pipeline, multi-layer cladding should be performed to meet the thickness requirement. When multi-layer cladding is required, except for the last layer, the cladding surface needs to be post-heat treated after each layer of cladding and then polished to remove slag and spatter.
[0040] S4. After the surfacing is completed, heat treatment is carried out and non-destructive testing is passed, and the surfacing process is completed.
[0041] The outer wall cladding process of the pipe provided by the present invention will be further described below by taking the pipe of a VDF cracking furnace as an example in conjunction with the accompanying drawings.
[0042] Example
[0043] The base material of the VDF cracking furnace pipeline is N6 pure nickel, and the size before welding is 108×4mm. Before welding, the welding area of the outer wall of the pipeline is strictly derusted, dehumidified, degreased and decontaminated by grinding and cleaning, and 100% MT magnetic particle inspection is carried out, and it meets the requirements of JB / T 4730.4-2011 and reaches Class I qualification.
[0044] The welding material used in the welding process is flux-cored welding wire, model TFW-625 (ENiCrMo-3), specification Φ1.2mm; the cladding thickness is 4.5mm, and the effective thickness is 4mm; the shielding gas used is industrial-grade purity CO2.
[0045] The first layer of cladding is performed on the welding area of the outer wall of the pipeline, and the corresponding specification parameters are shown in Table 1. The welding process adopts small line energy and narrow welds, and its heat input is strictly controlled. During welding, the furnace tube is controlled by CNC equipment to rotate and translate smoothly and at a steady speed. The welding equipment is cladding at a fixed position, and the inclination angle between the welding wire and the pipeline surface is controlled to be 65°. After the first layer of cladding is completed, the cladding surface is post-heat treated at (100-350)℃×2h, the purpose of which is to ensure slow cooling of the pipeline after welding and to eliminate hydrogen to a certain extent. Since there will be a certain amount of spatter during the CO2 gas shielded welding process, the surface forming of the cladding surface will be deteriorated after welding. Therefore, a certain amount of grinding is performed after the post-heat treatment, the main purpose of which is to remove slag and spatter. If the equipment factors cause the local overlap of the weld bead on the entire cladding surface to be small, resulting in the unevenness of the two joints>1mm affecting the overall, it should be corrected by grinding, which has no effect on the overall cladding.
[0046] Table 1 Process parameters of the first layer of CO2 gas shielded flux-cored wire cladding
[0047]
[0048] Table 2 Process parameters of the second layer of CO2 gas shielded flux-cored wire cladding
[0049]
[0050] The corresponding specification parameters for the second layer of cladding are shown in Table 2. During the second layer of cladding, the heat input of the weld and the temperature between passes must be strictly controlled to be ≤200°C. When the temperature is too high, welding is stopped and welding is resumed after natural cooling. In order to control the thickness of the cladding layer, the inclination angle between the welding wire and the pipe surface is adjusted to 75°.
[0051] The welded pipes were subjected to non-destructive testing after welding. The surface of the weld layer was tested by penetration method, and it reached the level I qualification according to the requirements of JB / T4730.5-2011; the joint surface of the welded layer and the pipe base material was tested by ultrasonic wave, and it reached the level I qualification according to the requirements of JB / T4730.3-2011. After testing, the welded layer of the VDF cracking furnace pipeline had no defects and was completely qualified.
[0052] Figure 7 It is the metallographic diagram of the VDF cracking furnace pipeline sample after cladding and the corresponding microscopic crystal arrangement. Figure 7 (a) shows the metallographic diagram and crystal arrangement of section A. Figure 7 (b) shows the metallographic image and crystal arrangement of section B. Figure 7 (c) shows the metallographic image of the C section (the outer cladding surface of the pipe). Figure 7 (d) shows the metallographic image of the D section (inner wall of the pipe). Figure 7(e) shows the arrangement of columnar crystals in the pipe after surfacing. Figure 7 (f) shows the stress condition of columnar crystals in the surfacing layer under axial stress after surfacing. Figure 7 (g) shows the stress condition of columnar crystals in the surfacing layer under hoop stress after surfacing.
[0053] like Figure 7 As shown, the VDF cracking furnace tube after surfacing in Example 1 was cut and sampled, and a metallographic sample was prepared and observed through an optical microscope. It was concluded that the columnar crystal distribution of the VDF cracking furnace pipeline surfacing layer obtained by the surfacing process provided by the present invention has an obvious regularity of uniform distribution along the wall thickness, and the stress condition of the VDF cracking furnace pipeline after surfacing under the conditions of circumferential and axial loads is more reasonable, and the mechanical properties are more excellent.
[0054] Under the same specifications and the same working conditions, the actual service life of the N6 pipeline of the VDF cracking furnace that is not processed by the pipeline outer wall cladding process provided by the present invention is about 2 to 3 years; the mechanical property test evaluation of the N6 pipeline of the VDF cracking furnace processed by the pipeline outer wall cladding process provided by the present invention extends its service life to about 10 years. Therefore, the pipeline outer wall cladding process provided by the present invention greatly improves the mechanical properties and economic benefits of the VDF cracking furnace.
[0055] The present invention mainly relies on the process implementation process itself to regulate the arrangement of microscopic crystals in the pipeline cladding layer, and has no special requirements for the selection of cladding materials. Therefore, this cladding process is also applicable to other forms of furnace pipes, and cladding materials are selected for processing based on their materials.
[0056] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. A pipeline outer wall cladding process, characterized in that: Applied to VDF cracking furnace pipelines; In the vertical force direction under the action of axial force, the VDF cracking furnace pipeline has more columnar crystal ternary intersection nodes. As the main stress-bearing site, the crystal intersection nodes are prone to stress concentration and are very likely to cause damage and creep holes. With the further evolution of the damage, wedge-shaped cracks are generated at the grain boundaries / subgrain boundaries parallel to the force direction; in the vertical force direction under the action of circumferential force, the VDF cracking furnace pipeline has longer grain boundaries and relatively fewer ternary intersection points. Part of the stress is shared at the grain boundaries. Under the same external load, the local stress is small, and the long grain boundaries will limit the expansion of creep holes at the grain boundaries. However, due to the presence of more non-columnar crystals in its microstructure, the length of the grain boundaries in the vertical force direction is not uniform, which is still prone to local stress concentration; By analyzing the stress conditions of the micro grain boundaries of the VDF cracking furnace pipeline under the conditions of large pipeline hoop force and axial force in actual working conditions, it is concluded that the optimal microstructure is a microstructure morphology composed entirely of columnar crystals distributed along the wall thickness direction. The optimal microstructure enables the stress state of the grain boundaries of the pipeline material to be maintained in a state of uniform distribution along the long grain boundaries at the hoop stress and axial stress with large loads, thereby reducing stress concentration. During the welding process, each wire welding will form a columnar crystal microstructure in the same direction as the welding wire, and its microstructure is completely composed of columnar crystals. The microstructure morphology composed entirely of columnar crystals distributed along the wall thickness direction is used as the processing technology of the VDF cracking furnace pipeline, which includes the following steps: S1. The welding area of the outer wall of the pipeline with the base material of N6 pure nickel was derusted, dehumidified, degreased and non-destructively tested. The welding material was flux-cored wire, model TFW-625 (ENiCrMo-3), diameter 1.2mm, cladding thickness 4.5mm, effective thickness 4mm, and the shielding gas used was industrial-grade purity CO2; S2. Adopt the form of outer wall cladding. After the pipeline is preheated, the welding is performed by keeping the welding gun in the same position and manipulating the pipeline to rotate continuously and move axially. During the welding process, the pipeline is regulated to rotate and translate smoothly and at a steady speed. The welding equipment is cladding at a fixed position. The welding wire forms an inclination angle with the pipeline surface to achieve the regulation of the internal structure of the cladding layer of the pipeline. Among them, when the first layer of cladding is performed on the welding area of the outer wall of the pipeline, the preheating temperature is ≥120℃, the interpass temperature is 80-300℃, and the inclination angle between the welding wire and the pipeline surface is controlled to be 65°. After the first layer of cladding is completed, the cladding surface is subjected to post-heat treatment of (100-350)℃×2h. When the second layer of cladding is performed, the heat input of the weld pass and the interpass temperature are strictly controlled to be ≤200℃, and the inclination angle between the welding wire and the pipeline surface is adjusted to 75°. S3. When welding multiple layers, except for the last layer, the weld surface needs to be post-heat treated after each layer and then polished to remove slag and spatter; S4. After the surfacing is completed, heat treatment is carried out and non-destructive testing is passed, and the surfacing process is completed.
2. The pipeline outer wall cladding process according to claim 1 is characterized in that: In step S2, the welding direction is from one end of the pipe to the other end along a spiral trajectory.
Citation Information
Patent Citations
Preparation method and application of composite pipe
CN113864537A