A high temperature resistant and corrosion resistant battery connection cable
By compounding modified rubber and butadiene rubber to form a dense protective layer, and combining it with fluoroplastic and silicone resin layers to coat metal conductors, the problems of poor mechanical properties and insufficient corrosion resistance of existing cables are solved, and the problem of high temperature and acid-base environments is achieved. Improved stability and performance.
Patent Information
- Application Number
- CN202310858863.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-13
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-07-13
AI Technical Summary
Existing high-temperature and anti-corrosion cables have poor mechanical properties, are not corrosion-resistant, and have insufficient stability in high-temperature environments.
Modified rubber is used as the outer sheath material. Potassium titanate whiskers, silica, aluminum dihydrogen phosphate and other compounds are compounded with butadiene rubber to form a dense protective layer, enhance hydrophobicity and cross-linked network, and combine with fluoroplastics and a silicone layer that coats the metal conductor to improve the mechanical properties and corrosion resistance of the cable.
It significantly improves the mechanical properties, high temperature resistance and corrosion resistance of the cable, making it stable in harsh environments such as high temperature and acid and alkali, and is suitable for battery connection cables and other fields.
Smart Images

Figure BDA0004336912650000121 
Figure BDA0004336912650000131
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of power transmission cables, and in particular to a high temperature resistant and corrosion resistant battery connection cable. Background Art
[0002] At present, the existing technologies of high temperature resistant and corrosion resistant battery connection cables mainly include copper core fluoroplastic cables. The core wire of this cable is made of copper, and the insulation layer is made of fluoroplastic. It has good high temperature resistance and corrosion resistance, and is suitable for power transmission in high temperature and acid-base corrosion environments. Polyimide cable, this cable uses polyimide as the insulation material, has good high temperature resistance and corrosion resistance, and is suitable for power transmission in harsh environments such as high temperature and chemical corrosion. Silicone rubber cable, this cable uses silicone rubber as the insulation material and sheath material, has good high temperature resistance and corrosion resistance, and is suitable for power transmission in high temperature and acid-base corrosion environments. Fluororubber cable, this cable uses fluororubber as the insulation material and sheath material, has good high temperature resistance and corrosion resistance, and is suitable for power transmission in high temperature and acid-base corrosion environments. Siloxane cable, this cable uses silicone as the insulation material and sheath material, has good high temperature resistance and corrosion resistance, and is suitable for power transmission in high temperature and acid-base corrosion environments. Polytetrafluoroethylene cable, this cable uses polytetrafluoroethylene as the insulation material and sheath material, has excellent high temperature resistance and corrosion resistance, and is suitable for power transmission in harsh environments such as high temperature and chemical corrosion.
[0003] In summary, the insulation and sheath materials mainly used in existing high temperature resistant and corrosion resistant battery connection cables include fluoroplastics, silicone rubber, polyimide, fluororubber, siloxane and polytetrafluoroethylene, etc., and various additives and fillers are added to improve their performance.
[0004] The various additives and fillers added to high temperature resistant and corrosion resistant battery connection cables mainly include vulcanizers, peroxides, plasticizers, antioxidants, heat stabilizers, silica, carbon black, titanium dioxide, etc. However, the use of these additives also has the disadvantages of low fluidity during processing, poor mechanical properties and high temperature resistance of the prepared cables, and easy aging and corrosion.
[0005] The invention patent CN105845246B discloses a flame retardant and high temperature resistant cable, including a copper conductor, an insulating layer coated on the outside of the copper conductor, a silicone wire sheath coated on the outside of the insulating layer, and an outer sheath coated on the outside of the silicone wire sheath; the outer sheath is made of a natural rubber composite material, and the raw materials of the natural rubber composite material include: natural rubber, EPDM rubber, butyl rubber, nylon 66, epoxy resin, stearic acid, zinc oxide, sulfur, di-tert-butyl peroxide isopropylbenzene, N,N′-m-phenylene bismaleimide, montmorillonite, kaolin, talcum powder, zinc borate, aluminum hydroxide, accelerator MBTS, accelerator DPG, accelerator CBS, antioxidant, phosphorus-containing flame retardant. The flame retardant and high temperature resistant cable proposed in the invention has high strength, good high temperature resistance and aging resistance, and excellent flame retardant performance. However, the flame retardant and high temperature resistant cable prepared by the invention has poor mechanical properties and unsatisfactory corrosion resistance. Summary of the invention
[0006] In view of the shortcomings of the cables in the prior art, such as poor mechanical properties, corrosion resistance and high temperature resistance, the technical problem to be solved by the present invention is to provide a battery connection cable with good mechanical properties, corrosion resistance and high temperature resistance.
[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0008] A high temperature resistant and corrosion resistant battery connection cable comprises the following components from the inside to the outside: a metal conductor, a fluoroplastic insulation layer, a silicone wire sheath, and an outer sheath; the raw materials of the outer sheath include: modified rubber, EPDM rubber, polytetrafluoroethylene, nylon 66, acrylic resin, stearic acid, heat stabilizer, UV protection agent, plasticizer, filler, and antioxidant.
[0009] Preferably, the raw materials of the outer sheath include, by weight: 60-100 parts of modified rubber, 10-30 parts of EPDM rubber, 10-30 parts of polytetrafluoroethylene, 10-20 parts of nylon 66, 10-20 parts of acrylic resin, 0.5-2 parts of stearic acid, 1-2 parts of heat stabilizer, 0.5-2 parts of UV inhibitor, 1-5 parts of plasticizer, 8-12 parts of filler, and 1-3 parts of antioxidant.
[0010] The preparation method of the outer sheath is as follows:
[0011] Step 1, weighing each raw material according to weight, uniformly mixing the modified rubber, EPDM rubber, polytetrafluoroethylene, nylon 66, acrylic resin and filler at a speed of 100 to 1000 rpm for 5 to 30 minutes to obtain a mixture A;
[0012] Step 2, adding stearic acid and plasticizer to the mixture A prepared in step 1, stirring and mixing at a speed of 100 to 1000 rpm for 5 to 30 minutes to obtain a mixture B;
[0013] Step 3, adding a heat stabilizer, an ultraviolet light blocking agent, and an antioxidant to the mixture B prepared in step 2, stirring and mixing at a speed of 100 to 1000 rpm for 10 to 50 minutes to obtain a mixture C;
[0014] Step 4, extruding and granulating the mixed material C prepared in step 3 using conventional processes in the art to obtain a cable material;
[0015] Step 5: melt and extrude the cable material prepared in step 4, and after cooling and solidification, obtain an outer sheath.
[0016] A preparation method of a high-temperature resistant and corrosion-resistant battery connection cable comprises the following steps: coating a metal conductor with a fluoroplastic insulation layer, coating a silicone wire sheath on the fluoroplastic insulation layer, and coating an outer sheath on the silicone wire sheath to obtain a high-temperature resistant and corrosion-resistant battery connection cable, wherein the diameter of the metal conductor is 1 to 5 mm; the thickness of the fluoroplastic insulation layer is 1 to 3 mm; the thickness of the silicone wire sheath is 3 to 8 mm; and the thickness of the outer sheath is 3 to 20 mm.
[0017] The preparation method of the modified rubber is as follows:
[0018] S1. Add potassium titanate whiskers and silicon dioxide into Tris-HCl buffer, stir and mix, disperse by ultrasonication, add 1,10-decanediol diacrylate and dopamine hydrochloride aqueous solution, stir at high temperature, centrifuge, collect the precipitate, wash, dry, grind into powder, and sieve to obtain a mixture;
[0019] S2, adding the mixture prepared in step S1 into liquid aluminum dihydrogen phosphate and stirring, then centrifuging, collecting the solid, and drying to obtain a composite agent;
[0020] S3. At high temperature, stir and mix the butadiene rubber, the composite agent prepared in step S2, N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine, zinc oxide and stearic acid; then lower the temperature, add sulfur powder and N-cyclohexyl-2-benzothiazolesulfenamide, stir, and vulcanize to obtain a modified rubber.
[0021] Preferably, the preparation method of the modified rubber is as follows, in parts by weight:
[0022] S1. Add 4 to 8 parts of potassium titanate whiskers and 20 to 30 parts of silicon dioxide to 200 to 400 parts of Tris-HCl buffer, stir and mix at 800 to 1200 rpm for 1 to 3 minutes, and ultrasonically disperse for 20 to 40 minutes. The ultrasonic power is 200 to 400 W and the ultrasonic frequency is 40 to 100 kHz. Add 4 to 8 parts of 1,10-decanediol diacrylate and 10 to 30 parts of 40 to 60 g / L dopamine hydrochloride aqueous solution, stir at 50 to 70° C. and 100 to 300 rpm for 10 to 30 hours, and then centrifuge at 5000 to 15000 rpm for 3 to 20 minutes, collect the precipitate, wash it with anhydrous ethanol for 1 to 3 times, vacuum dry it at 50 to 70° C. for 5 to 20 hours, and then grind it into powder, and pass it through a 100 to 400 mesh sieve to obtain a mixture;
[0023] S2, adding the mixture prepared in step S1 to 150-300 parts of liquid aluminum dihydrogen phosphate and stirring at 100-300 rpm for 10-30 min, then centrifuging at 5000-15000 rpm for 3-20 min, collecting the solid, and vacuum drying at 50-70° C. for 5-20 h to obtain a composite agent;
[0024] S3, at 80-120° C., 80-120 parts of butadiene rubber, the composite agent prepared in step S2, 4-8 parts of N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine, 1-3 parts of zinc oxide and 0.5-2 parts of stearic acid are stirred and mixed at 100-300 rpm for 5-10 min; then the temperature is adjusted to 60-100° C., 0.5-2 parts of sulfur powder and 0.5-2 parts of N-cyclohexyl-2-benzothiazolesulfenamide are added, stirred at 100-300 rpm for 10-50 min, and vulcanized in a vulcanizer at 130-150° C. and 13-17 MPa for 10-20 min to obtain a modified rubber.
[0025] Preferably, the UV blocker is at least one of the UV absorbers UV-326, UV-327, UV-328, UV-531, and UV-541.
[0026] The heat stabilizer is a sulfur-containing heat stabilizer.
[0027] Preferably, the sulfur-containing heat stabilizer is at least one of diphenyl disulfide, dioctyl disulfide, mercaptoethanol, mercaptopropanol, isopropyl mercaptan, diphenyl sulfide, dioctyl sulfide, and isooctyl sulfide.
[0028] The plasticizer is at least one of phthalates, epoxidized lipids, and alkyd esters.
[0029] Preferably, the plasticizer is at least one of di(2-ethylhexyl) phthalate and dibutyl phthalate.
[0030] The filler is at least one of carbon fiber, montmorillonite, kaolin, alumina powder, talc powder and perlite.
[0031] Preferably, the filler is a mixture of alumina powder, talc powder and perlite in a mass ratio of 1-3:4-6:2-4.
[0032] The antioxidant is at least one of 2,6-di-tert-butyl-p-cresol, tri-tert-butyl-hydroxybenzene, and 2,2'-dihydroxy-4,4'-dimethylbenzophenone.
[0033] The invention comprises the following steps of stirring and mixing modified rubber, EPDM rubber, polytetrafluoroethylene, nylon 66, acrylic resin, alumina powder, talcum powder and perlite to obtain a mixture A; then adding stearic acid and di(2-ethylhexyl) phthalate, stirring and mixing to obtain a mixture B; then adding diphenyl disulfide and 2,6-di-tert-butyl-p-cresol, stirring and mixing to obtain a mixture C; extruding and granulating by a conventional process in the art to obtain a cable material; then melt-extruding, cooling and solidifying to obtain an outer sheath; and coating a fluoroplastic insulating layer on the outside of a metal conductor, coating a silicone wire sheath on the outside of the fluoroplastic insulating layer, and coating an outer sheath on the outside of the silicone wire sheath to obtain a high temperature resistant and corrosion resistant battery connection cable.
[0034] The modified rubber is prepared by adding potassium titanate whiskers and silicon dioxide into a Tris-HCl buffer solution, stirring and mixing, ultrasonically dispersing, adding 1,10-decanediol diacrylate and a dopamine hydrochloride aqueous solution, stirring at high temperature, centrifuging, washing, drying, grinding, and sieving to obtain a mixture; adding the mixture into liquid aluminum dihydrogen phosphate, stirring, centrifuging, and drying to obtain a composite agent; mixing butadiene rubber, the composite agent, N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine, zinc oxide, and stearic acid at high temperature; adding sulfur powder and N-cyclohexyl-2-benzothiazolesulfenamide, stirring, and vulcanizing to obtain the modified rubber.
[0035] Dopamine hydrochloride can enhance the interaction between filler and rubber interface. Silica is added to the rubber network as a macromolecular free radical by treating 1,10-decanediol diacrylate and dopamine hydrochloride aqueous solution to promote the formation of chemical cross-linked network in rubber. The uniformity of the rubber cross-linked network is changed by filling, and the tensile properties are affected by forming physical cross-linking sites by adsorbing chains. The cross-linking and adsorption of chains form a non-ideal network to prevent large-scale slippage of chains in the network, reduce the interface between filler and rubber and the molecular network defects that may cause damage under high strain, and enhance the mechanical properties and thermal stability of the cable. A dense protective layer is formed in butadiene rubber by introducing potassium titanate whiskers, 1,10-decanediol diacrylate, aluminum dihydrogen phosphate, N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine, zinc oxide and stearic acid. The introduction of 1,10-decanediol diacrylate is conducive to promoting the formation of crystal nuclei. The more crystal nuclei there are, the finer the size of the crystals, and the denser the protective layer obtained. The protective layer can block the invasion of corrosive media and protect the rubber. 1,10-decanediol diacrylate is hydrophobic. During the coating formation process, potassium titanate whiskers treated with 1,10-decanediol diacrylate are gradually deposited with aluminum dihydrogen phosphate, making the final protective layer super hydrophobic. During the corrosion process, when the cable comes into contact with corrosive liquids, the lotus effect of the super hydrophobic coating will produce an entrapped air layer in the structure to isolate corrosive ions, thereby enhancing its corrosion resistance for long-term use.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] 1) The present invention adds compounds such as aluminum dihydrogen phosphate, potassium titanate and silicon dioxide to compound with butadiene rubber to obtain modified rubber, which can effectively improve the mechanical properties of the rubber such as strength, hardness and wear resistance.
[0038] 2) The present invention adds potassium titanate whiskers, silicon dioxide and aluminum dihydrogen phosphate, which can effectively improve the high temperature resistance and aging resistance of the rubber, so that it can maintain stable performance in a high temperature environment.
[0039] 3) The present invention forms a dense protective layer in butadiene rubber by using potassium titanate whiskers, 1,10-decanediol diacrylate, aluminum dihydrogen phosphate, N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine, zinc oxide and stearic acid to enhance hydrophobicity, which can effectively improve the corrosion resistance and chemical resistance of the rubber and enable it to maintain stable performance in corrosive environments such as acids and alkalis.
[0040] 4) The present invention can obtain an outer sheath with excellent mechanical properties, high temperature resistance and corrosion resistance through the preparation of modified rubber, and can be widely used in the fields of battery connection cables and the like. DETAILED DESCRIPTION
[0041] Main sources of substances:
[0042] The fluoroplastic insulating layer in the embodiment is made of PEA with a brand number of 440HPAX produced by DuPont of the United States and is prepared by conventional technology.
[0043] Silicone wire sheath: Guangdong Shengpai Insulation Materials Co., Ltd., item number: BQG1.5kv.
[0044] Potassium titanate whiskers: Shanghai Kaishefeng Industrial Co., Ltd., item number: 2010021.
[0045] Silica: Particle size: 20nm.
[0046] Tris-HCl buffer: pH: 8.5.
[0047] Liquid aluminum dihydrogen phosphate, Shandong Zhelong Biotechnology Co., Ltd., item number: 84.
[0048] Ultraviolet absorber UV-326, Hunan Muyang New Materials Co., Ltd., model: UV-326.
[0049] Butadiene rubber: Shanghai Huanyang Chemical Technology Co., Ltd., model: THIXON OSN-2-EF-V.
[0050] Zinc powder: Particle size: 800 mesh.
[0051] Magnesium powder: particle size: 200 mesh.
[0052] EPDM rubber: Shanghai Gaoming Chemical Co., Ltd., brand number: 162257.
[0053] Polytetrafluoroethylene: Dongguan Jingtian Plastic Raw Materials Co., Ltd., brand: JH300.
[0054] Acrylic resin: Hanbot Paint (Shandong) Co., Ltd., brand: hbt.
[0055] Talc: Particle size: 2000 mesh.
[0056] Perlite: Particle size: 200 mesh.
[0057] Example 1
[0058] A preparation method for a high-temperature resistant and corrosion-resistant battery connection cable comprises the following steps: coating a copper conductor with a fluoroplastic insulation layer, coating the fluoroplastic insulation layer with a silicone wire sheath, and coating the silicone wire sheath with an outer sheath to obtain a high-temperature resistant and corrosion-resistant battery connection cable, wherein the thickness of the silicone wire sheath is 4.8 mm; the thickness of the outer sheath is 8 mm; the diameter of the copper conductor is 3 mm; and the thickness of the fluoroplastic insulation layer is 2 mm.
[0059] The preparation method of the outer sheath is as follows:
[0060] Step 1, 80kg of modified rubber, 20kg of EPDM rubber, 20kg of polytetrafluoroethylene, 15kg of nylon 66, 15kg of acrylic resin, 2kg of alumina powder, 5kg of talc powder, and 3kg of perlite are uniformly mixed at a speed of 500rpm for 20min to obtain a mixture A;
[0061] Step 2: Add 1 kg of stearic acid and 3 kg of di(2-ethylhexyl) phthalate to the mixture A prepared in step 1, and stir and mix at 500 rpm for 20 min to obtain a mixture B;
[0062] Step 3, adding 1.5 kg of diphenyl disulfide, 1 kg of ultraviolet absorber UV-326, and 2 kg of 2,6-di-tert-butyl-p-cresol to the mixed material B prepared in step 2, and stirring and mixing at a speed of 500 rpm for 30 minutes to obtain a mixed material C;
[0063] Step 4, extruding and granulating the mixed material C prepared in step 3 using conventional processes in the art to obtain a cable material;
[0064] Step 5: melt and extrude the cable material prepared in step 4, and after cooling and solidification, obtain an outer sheath.
[0065] The preparation method of the modified rubber is as follows:
[0066] S1. Add 6 g potassium titanate whisker and 25 g silicon dioxide to 300 g Tris-HCl buffer, stir and mix at 1000 rpm for 2 min, and ultrasonically disperse for 30 min, with an ultrasonic power of 300 W and an ultrasonic frequency of 50 kHz. Add 6 g 1,10-decanediol diacrylate and 20 g 50 g / L dopamine hydrochloride aqueous solution, stir at 200 rpm at 60° C. for 24 h, and then centrifuge at 8000 rpm for 10 min. Collect the precipitate, wash it with anhydrous ethanol three times, dry it in vacuum at 60° C. for 12 h, and then grind it into powder, and pass it through a 300-mesh sieve to obtain a mixture.
[0067] S2, adding the mixture prepared in step S1 to 200 g of liquid aluminum dihydrogen phosphate and stirring at 200 rpm for 20 min, then centrifuging at 8000 rpm for 10 min, collecting the solid, and vacuum drying at 60° C. for 12 h to obtain a composite agent;
[0068] S3. At 100°C, 100g of butadiene rubber, the composite agent prepared in step S2, 6g of N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine, 2g of zinc oxide and 1g of stearic acid were stirred at 200rpm for 8min; then the temperature was adjusted to 80°C, 1g of sulfur powder and 1g of N-cyclohexyl-2-benzothiazolesulfenamide were added, and the mixture was stirred at 200rpm for 30min. The mixture was vulcanized in a vulcanizer at 140°C and 15MPa for 15min to obtain a modified rubber.
[0069] Example 2
[0070] A method for preparing a high temperature resistant and corrosion resistant battery connection cable is substantially the same as that in Example 1, with the only difference being that the preparation method of the modified rubber is different.
[0071] The preparation method of the modified rubber is as follows:
[0072] S1. Add 6 g potassium titanate whisker and 25 g silicon dioxide to 300 g Tris-HCl buffer, stir and mix at 1000 rpm for 2 min, ultrasonically disperse for 30 min, with an ultrasonic power of 300 W and an ultrasonic frequency of 50 kHz, add 20 g 50 g / L dopamine hydrochloride aqueous solution, stir at 200 rpm at 60 ° C for 24 h, then centrifuge at 8000 rpm for 10 min, collect the precipitate, wash with anhydrous ethanol 3 times, vacuum dry at 60 ° C for 12 h, then grind into powder, and pass through a 300 mesh sieve to obtain a mixture;
[0073] S2, adding the mixture prepared in step S1 to 200 g of liquid aluminum dihydrogen phosphate and stirring at 200 rpm for 20 min, then centrifuging at 8000 rpm for 10 min, collecting the solid, and vacuum drying at 60° C. for 12 h to obtain a composite agent;
[0074] S3. At 100°C, 100g of butadiene rubber, the composite agent prepared in step S2, 6g of N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine, 2g of zinc oxide and 1g of stearic acid were stirred at 200rpm for 8min; then the temperature was adjusted to 80°C, 1g of sulfur powder and 1g of N-cyclohexyl-2-benzothiazolesulfenamide were added, and the mixture was stirred at 200rpm for 30min. The mixture was vulcanized in a vulcanizer at 140°C and 15MPa for 15min to obtain a modified rubber.
[0075] The preparation method of the outer sheath is the same as that of Example 1.
[0076] Example 3
[0077] A method for preparing a high temperature resistant and corrosion resistant battery connection cable is substantially the same as that in Example 1, with the only difference being that the preparation method of the modified rubber is different.
[0078] The preparation method of the modified rubber is as follows:
[0079] S1. Add 6 g potassium titanate whisker and 25 g silicon dioxide to 300 g Tris-HCl buffer, stir and mix at 1000 rpm for 2 min, and ultrasonically disperse for 30 min. The ultrasonic power is 300 W and the ultrasonic frequency is 50 kHz. Add 6 g 1,10-decanediol diacrylate, stir at 200 rpm at 60°C for 24 h, and then centrifuge at 8000 rpm for 10 min. Collect the precipitate, wash it with anhydrous ethanol three times, vacuum dry it at 60°C for 12 h, and then grind it into powder, and pass it through a 300-mesh sieve to obtain a mixture.
[0080] S2, adding the mixture prepared in step S1 to 200 g of liquid aluminum dihydrogen phosphate, stirring at 200 rpm for 20 min, then centrifuging at 8000 rpm for 10 min, collecting the solid, and vacuum drying at 60° C. for 12 h to obtain a composite agent;
[0081] S3. At 100°C, 100g of butadiene rubber, the composite agent prepared in step S2, 6g of N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine, 2g of zinc oxide and 1g of stearic acid were stirred at 200rpm for 8min; then the temperature was adjusted to 80°C, 1g of sulfur powder and 1g of N-cyclohexyl-2-benzothiazolesulfenamide were added, and the mixture was stirred at 200rpm for 30min. The mixture was vulcanized in a vulcanizer at 140°C and 15MPa for 15min to obtain a modified rubber.
[0082] The preparation method of the outer sheath is the same as that of Example 1.
[0083] Example 4
[0084] A method for preparing a high temperature resistant and corrosion resistant battery connection cable is substantially the same as that in Example 1, with the only difference being that the preparation method of the modified rubber is different.
[0085] The preparation method of the modified rubber is as follows:
[0086] S1. Add 6 g potassium titanate whisker and 25 g silicon dioxide to 300 g Tris-HCl buffer, stir and mix at 1000 rpm for 2 min, and ultrasonically disperse for 30 min, with an ultrasonic power of 300 W and an ultrasonic frequency of 50 kHz. Add 6 g 1,10-decanediol diacrylate and 20 g 50 g / L dopamine hydrochloride aqueous solution, stir at 200 rpm at 60° C. for 24 h, and then centrifuge at 8000 rpm for 10 min. Collect the precipitate, wash it with anhydrous ethanol three times, dry it in vacuum at 60° C. for 12 h, and then grind it into powder, and pass it through a 300-mesh sieve to obtain a mixture.
[0087] S2. At 100°C, 100g of butadiene rubber, the mixture prepared in step S1, 6g of N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine, 2g of zinc oxide and 1g of stearic acid were stirred at 200rpm for 8min; then the temperature was adjusted to 80°C, 1g of sulfur powder and 1g of N-cyclohexyl-2-benzothiazolesulfenamide were added, and the mixture was stirred at 200rpm for 30min. The mixture was vulcanized in a vulcanizer at 140°C and 15MPa for 15min to obtain a modified rubber.
[0088] The preparation method of the outer sheath is the same as that of Example 1.
[0089] Comparative Example 1
[0090] A method for preparing a high temperature resistant and corrosion resistant battery connection cable is substantially the same as that in Example 1, with the only difference being that the preparation method of the modified rubber is different.
[0091] The preparation method of the modified rubber is as follows:
[0092] S1. Add 6 g potassium titanate whisker and 25 g silicon dioxide to 300 g Tris-HCl buffer, stir and mix at 1000 rpm for 2 min, ultrasonically disperse for 30 min, with an ultrasonic power of 300 W and an ultrasonic frequency of 50 kHz, then centrifuge at 8000 rpm for 10 min, collect the precipitate, wash with anhydrous ethanol three times, vacuum dry at 60° C. for 12 h, then grind into powder, and pass through a 300-mesh sieve to obtain a mixture;
[0093] S2. At 100°C, 100g of butadiene rubber, the mixture prepared in step S1, 6g of N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine, 2g of zinc oxide and 1g of stearic acid were stirred at 200rpm for 8min; then the temperature was adjusted to 80°C, 1g of sulfur powder and 1g of N-cyclohexyl-2-benzothiazolesulfenamide were added, and the mixture was stirred at 200rpm for 30min. The mixture was vulcanized in a vulcanizer at 140°C and 15MPa for 15min to obtain a modified rubber.
[0094] The preparation method of the outer sheath is the same as that of Example 1.
[0095] Comparative Example 2
[0096] A method for preparing a high temperature resistant and corrosion resistant battery connection cable is substantially the same as that in Example 1, with the only difference being that the modified rubber is replaced with an equal amount of butadiene rubber.
[0097] Test Example 1
[0098] Tensile properties test
[0099] The test was conducted on an Instron 869 electronic universal testing machine. The test was based on the standard GB / T1040-2006 "Determination of tensile properties of plastics". The cable material prepared in step 4 was processed into 1BA type specimens for testing. The tensile speed was 5mm / min. Five samples were tested as a group, and the final result was the average of the test data of the five samples. The test results are shown in Table 1.
[0100] Table 1: Tensile properties test results
[0101] Trial plan Tensile strength(MPa) Elongation at break (%) Example 1 84.6 18.2 Example 2 76.3 15.8 Example 3 75.8 15.6 Example 4 83.7 17.9 Comparative Example 1 72.1 14.6 Comparative Example 2 69.4 12.5
[0102] Test Example 2
[0103] High temperature resistance test
[0104] The cable material prepared in step 4 of the present invention was ground into powder, 5 mg was weighed and placed in a ceramic crucible, and the thermal weight loss starting temperature in air was tested by a thermal gravimetric analyzer. The test temperature range was 40-1000°C, the heating rate was 10, and the final 5% weight loss temperature and 10% weight loss temperature were obtained. Each group was tested three times and the average value was taken. The test results are shown in Table 2.
[0105] Table 2: High temperature resistance test results
[0106] Trial plan 5% weight loss temperature (℃ 10% weight loss temperature (℃ Example 1 351.7 432.4 Example 2 330.5 393.4 Example 3 331.4 393.9 Example 4 321.5 380.4 Comparative Example 1 309.5 356.3 Comparative Example 2 302.6 341.7
[0107] Test Example 3
[0108] Corrosion resistance test
[0109] The test was carried out using a WD-T-60 salt spray test machine. Refer to GB / T 1771-2007 "Determination of neutral salt spray resistance of paints and varnishes". The outer sheath prepared in step 5 was exposed to a salt spray test chamber, and the atomized test solution was sprayed into the test chamber. The salt spray settled evenly on the surface of the sample under the action of its own weight. The test solution contained 5wt% NaCl and 0.8wt% HCl by mass fraction, and the total solid content did not exceed 200×10 -6 , the pH range is 6.5~7.2, and the temperature in the salt spray chamber is kept constant at 35±1.℃. It is generally specified at 80cm 2 On the horizontal area, the average amount of salt spray is 2mL / h. When the sample is placed in the salt spray chamber, the main surface to be tested should be 15-30° to the vertical direction. The test time is 72h, and the corrosion state of the outer sheath surface is observed. The test results are shown in Table 3.
[0110] Table 3: Corrosion resistance test results
[0111]
[0112]
[0113] It can be seen from the test results of test examples 1 to 3 that embodiment 1 has the best comprehensive performance, which may be due to the fact that in embodiment 1 of the present invention, modified rubber, EPDM rubber, polytetrafluoroethylene, nylon 66, acrylic resin, alumina powder, talc powder and perlite are stirred and mixed to obtain a mixture A; stearic acid and di(2-ethylhexyl) phthalate are then added and stirred and mixed to obtain a mixture B; diphenyl disulfide and 2,6-di-tert-butyl-p-cresol are then added and stirred and mixed to obtain a mixture C; a cable material is obtained by extrusion granulation using a conventional process in the art; an outer sheath is obtained after melt extrusion and cooling and solidification; a high temperature resistant and corrosion resistant battery connection cable is obtained by coating a fluoroplastic insulation layer on the outside of a metal conductor, coating a silicone wire sheath on the outside of the fluoroplastic insulation layer, and coating an outer sheath on the outside of the silicone wire sheath.
[0114] The modified rubber is prepared by adding potassium titanate whiskers and silicon dioxide into a Tris-HCl buffer solution, stirring and mixing, ultrasonically dispersing, adding 1,10-decanediol diacrylate and a dopamine hydrochloride aqueous solution, stirring at high temperature, centrifuging, washing, drying, grinding, and sieving to obtain a mixture; adding the mixture into liquid aluminum dihydrogen phosphate, stirring, centrifuging, and drying to obtain a composite agent; mixing butadiene rubber, the composite agent, N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine, zinc oxide, and stearic acid at high temperature; adding sulfur powder and N-cyclohexyl-2-benzothiazolesulfenamide, stirring, and vulcanizing to obtain the modified rubber.
[0115] Dopamine hydrochloride can enhance the interaction between filler and rubber interface. Silica is added to the rubber network as a macromolecular free radical by treating 1,10-decanediol diacrylate and dopamine hydrochloride aqueous solution to promote the formation of chemical cross-linked network in rubber. The uniformity of the rubber cross-linked network is changed by filling, and the tensile properties are affected by forming physical cross-linking sites by adsorbing chains. The cross-linking and adsorption of chains form a non-ideal network to prevent large-scale slippage of chains in the network, reduce the interface between filler and rubber and the molecular network defects that may cause damage under high strain, and enhance the mechanical properties of the cable. A dense protective layer is formed in butadiene rubber by introducing potassium titanate whiskers, 1,10-decanediol diacrylate, aluminum dihydrogen phosphate, N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine, zinc oxide and stearic acid. The introduction of 1,10-decanediol diacrylate is conducive to promoting the formation of crystal nuclei. The more crystal nuclei there are, the finer the size of the crystals, and the denser the protective layer obtained. The protective layer can block the invasion of corrosive media and protect the rubber. 1,10-decanediol diacrylate is hydrophobic. During the coating formation process, potassium titanate whiskers treated with 1,10-decanediol diacrylate are gradually deposited with aluminum dihydrogen phosphate, making the final protective layer super hydrophobic. During the corrosion process, when the cable comes into contact with corrosive liquids, the lotus effect of the super hydrophobic coating will produce an entrapped air layer in the structure to isolate corrosive ions, thereby enhancing its corrosion resistance for long-term use.
Claims
1. A high temperature resistant and corrosion resistant battery connection cable, characterized in that: From inside to outside, it includes the following components: metal conductor, fluoroplastic insulation layer, silicone wire sheath, and outer sheath; The raw materials of the outer sheath include, by weight: 60-100 parts of modified rubber, 10-30 parts of EPDM rubber, 10-30 parts of polytetrafluoroethylene, 10-20 parts of nylon 66, 10-20 parts of acrylic resin, 0.5-2 parts of stearic acid, 1-2 parts of heat stabilizer, 0.5-2 parts of UV protection agent, 1-5 parts of plasticizer, 8-12 parts of filler, and 1-3 parts of antioxidant; The preparation method of the outer sheath is as follows: Step 1, weighing each raw material according to weight, uniformly mixing the modified rubber, EPDM rubber, polytetrafluoroethylene, nylon 66, acrylic resin and filler at a speed of 100 to 1000 rpm for 5 to 30 minutes to obtain a mixture A; Step 2, adding stearic acid and plasticizer to the mixture A prepared in step 1, stirring and mixing at a speed of 100 to 1000 rpm for 5 to 30 minutes to obtain a mixture B; Step 3, adding a heat stabilizer, an ultraviolet light blocking agent, and an antioxidant to the mixture B prepared in step 2, stirring and mixing at a speed of 100 to 1000 rpm for 10 to 50 minutes to obtain a mixture C; Step 4, extruding and granulating the mixed material C prepared in step 3 using conventional processes in the art to obtain a cable material; Step 5, melt and extrude the cable material prepared in step 4, and after cooling and solidification, obtain an outer sheath; The preparation method of the modified rubber is as follows: S1. Add potassium titanate whiskers and silicon dioxide into Tris-HCl buffer, stir and mix, disperse by ultrasonication, add 1,10-decanediol diacrylate and dopamine hydrochloride aqueous solution, stir at high temperature, centrifuge, collect the precipitate, wash, dry, grind into powder, and sieve to obtain a mixture; S2, adding the mixture prepared in step S1 into liquid aluminum dihydrogen phosphate and stirring, then centrifuging, collecting the solid, and drying to obtain a composite agent; S3, at high temperature, mixing butadiene rubber, the composite agent prepared in step S2, N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine, zinc oxide and stearic acid; then lowering the temperature, adding sulfur powder and N-cyclohexyl-2-benzothiazolesulfenamide, stirring, and vulcanizing to obtain a modified rubber; The anti-ultraviolet agent is at least one of the ultraviolet absorbers UV-326, UV-327, UV-328, UV-531, and UV-541; The heat stabilizer is a sulfur-containing heat stabilizer; The plasticizer is at least one of di(2-ethylhexyl)phthalate and dibutyl phthalate; The filler is at least one of carbon fiber, montmorillonite, kaolin, alumina powder, talc powder and perlite; The antioxidant is at least one of 2,6-di-tert-butyl-p-cresol, tri-tert-butyl-hydroxybenzene, and 2,2'-dihydroxy-4,4'-dimethylbenzophenone.
2. A method for preparing the high temperature resistant and corrosion resistant battery connection cable as claimed in claim 1, characterized in that: A fluoroplastic insulation layer is coated on the outside of a metal conductor, a silicone wire sheath is coated on the outside of the fluoroplastic insulation layer, and an outer sheath is coated on the outside of the silicone wire sheath, so as to obtain a high-temperature resistant and corrosion-resistant battery connection cable. The diameter of the metal conductor is 1 to 5 mm; the thickness of the fluoroplastic insulation layer is 1 to 3 mm; the thickness of the silicone wire sheath is 3 to 8 mm; and the thickness of the outer sheath is 3 to 20 mm.
Citation Information
Patent Citations
A flame retardant and high temperature resistant cable
CN105845246B
Nitrile rubber insulation flat cable material and preparation method
CN102746593A
Flame-retardant high-temperature-resistant cable
CN105845246A
Method for preparing silicone rubber gasket for electronic packaging heat dissipation by using methyl vinyl phenyl silicone rubber with high phenyl content
CN115505267A