Lubricating paint, lubricating coating and preparation method and application thereof

Through the combination of hyperbranched polysiloxane-modified molybdenum disulfide and sodium silicate and other components, a wear-resistant room-temperature curing lubricating coating is formed, which solves the problem in the existing technology of the resistance of molybdenum disulfide-based coatings in low-orbit space environments. The problem of insufficient atomic oxygen performance has been solved, and efficient lubrication treatment on the surface of large mechanical transmission friction pairs has been achieved.

CN116656159BActive Publication Date: 2024-10-18LANZHOU INST OF PHYSICS CHINESE ACADEMY OF SPACE TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310594370.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-10-18
Estimated Expiration
2043-05-24

AI Technical Summary

Technical Problem

The existing molybdenum disulfide-based solid lubricating coating has insufficient resistance to atomic oxygen in low-orbit space environments, and it is difficult to prepare a room-temperature curing coating on the surface of a large ring gear.

Method used

It uses components such as molybdenum disulfide, sodium silicate, sodium fluorosilicate and antimony trioxide modified with hyperbranched polysiloxane, and is processed through high-speed dispersion and zirconium oxide bead grinding to form a wear-resistant and curable material at room temperature. Lubricating coating, and forming a coating on the surface of large mechanical transmission friction pairs through spraying.

Benefits of technology

A room-temperature solidified lubricating coating with excellent atomic oxygen resistance and high wear resistance in low-orbit space environment has been realized, which is suitable for lubrication and anti-cold welding treatment of large mechanical transmission friction pairs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004246569870000041
    Figure BDA0004246569870000041
Patent Text Reader

Abstract

The present invention provides a lubricating paint, a lubricating coating and a preparation method and application thereof, and relates to the field of lubricating paint. The lubricating paint comprises a component A and a component B. By weight, the component A comprises: 50 to 150 parts of hyperbranched polysiloxane-modified molybdenum disulfide, 10 to 30 parts of antimony trioxide, 3 to 9 parts of dispersant, 3.8 to 11.4 parts of sodium fluorosilicate, and 223 to 668 parts of deionized water; the component B comprises: 100 to 300 parts of sodium silicate, and 66 to 200 parts of deionized water. On the one hand, the solid lubricant and the binder in the lubricating paint have good compatibility, and the solid lubricating coating prepared has a low vacuum friction coefficient, excellent wear resistance and load-bearing capacity, and excellent atomic oxygen resistance; on the other hand, the coating adopts a room temperature curing formula design, which can be sprayed on the surface of large movable parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of lubricating coatings, and in particular to a lubricating coating, a lubricating coating, and a preparation method and application thereof. Background Art

[0002] During the construction of my country's space station, a large gear ring and gear friction pair was designed. Due to the large size of the gear ring, it is difficult to prepare a bonded solid lubricating coating on its surface by thermal baking. In addition, since the part is serving in a low-orbit space environment, it is subject to atomic oxygen corrosion and has a long operating life. Therefore, a room-temperature curing lubricating coating with good atomic oxygen resistance and wear resistance is urgently needed.

[0003] Huo Lixia et al. (Surface Technology, 2014 (43), 111-115) studied the effect of substrate material on the tribological properties of sodium silicate bonded MoS2 solid lubricant coatings. However, this type of sodium silicate bonded MoS2 solid lubricant coating is a single-component high-temperature curing coating, and the MoS2 solid lubricant used has not been surface-modified with hyperbranched polysiloxane, making it difficult to use on large gear ring surfaces. Summary of the invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects of the prior art that the molybdenum disulfide-based solid lubricating coating has insufficient atomic oxygen resistance and that large mechanical moving parts are difficult to heat-bake and solidify, thereby providing a lubricating paint, a lubricating coating, and a preparation method and application thereof.

[0005] In a first aspect, the present invention provides a lubricating coating, comprising component A and component B, which are measured by weight.

[0006] The component A comprises: 50 to 150 parts of hyperbranched polysiloxane-modified molybdenum disulfide, 10 to 30 parts of antimony trioxide, 3 to 9 parts of a dispersant, 3.8 to 11.4 parts of sodium fluorosilicate, and 223 to 668 parts of deionized water;

[0007] The component B comprises: 100 to 300 parts of sodium silicate and 66 to 200 parts of deionized water.

[0008] Furthermore, the modulus of the sodium silicate is 3.1-3.4, and the solid content is 50%.

[0009] Furthermore, the preparation method of the hyperbranched polysiloxane-modified molybdenum disulfide is as follows:

[0010] 1) Mixing the silane coupling agent KH-580 with toluene to obtain a mixed solution, then adding molybdenum disulfide powder to the mixed solution, uniformly dispersing by ultrasonication, heating to reflux of toluene, stirring and keeping warm for more than 10 hours, cooling to room temperature after the insulation is completed, centrifuging, and washing the precipitate with toluene to obtain SH-MoS2 concentrated slurry;

[0011] 2) Mixing SH-MoS2 concentrated slurry, isobutyltriethoxysilane and neopentyl glycol, adding to a mixed solvent of toluene and N,N-dimethylformamide, stirring and raising the material temperature to 100±5°C and keeping warm, and distilling out the liquid; while ensuring that the distillation temperature does not exceed 78°C, continuously raising the material temperature to 160±5°C and keeping warm for more than 5 hours; after the insulation is completed, cooling to room temperature, centrifuging, washing the precipitate with toluene, and naturally drying to obtain a hyperbranched polysiloxane modified molybdenum disulfide powder,

[0012] In step 1), the total mass of the mixed solution is 100%, the mass fraction of KH-580 is 5% to 30%, and the mass fraction of toluene is 70% to 95%; the total mass of KH-580 and molybdenum disulfide powder is 100%, the mass fraction of KH-580 is 5% to 20%, and the mass fraction of molybdenum disulfide powder is 80% to 95%; the purity of the molybdenum disulfide powder is ≥98%, D 50 ≤1.5μm;

[0013] In step 2), taking the total mass of dry matter SH-MoS2, isobutyltriethoxysilane and neopentyl glycol in the SH-MoS2 concentrated slurry as 100%, the mass fraction of dry matter SH-MoS2 is 50% to 70%, the mass fraction of isobutyltriethoxysilane is 20% to 30%, and the mass fraction of neopentyl glycol is 10% to 20%; in the mixed solvent of toluene and N,N-dimethylformamide, the volume ratio of toluene and N,N-dimethylformamide is 1:1.

[0014] In a second aspect, the present invention provides a method for preparing the lubricating material, comprising the following steps:

[0015] The hyperbranched polysiloxane-modified molybdenum disulfide, antimony trioxide, dispersant, sodium fluorosilicate and deionized water are mixed in proportion, and the mixture is subjected to high-speed dispersion and grinding with zirconium oxide beads to obtain component A;

[0016] Mix sodium silicate and deionized water in proportion to obtain component B;

[0017] The component A and the component B are mixed evenly to obtain the lubricating material.

[0018] In a third aspect, the present invention provides a lubricating coating formed from the lubricating material described above, or the lubricating material obtained by the preparation method described above.

[0019] In a fourth aspect, the present invention provides a method for preparing the lubricating coating, comprising: spraying the lubricating coating on the surface to be treated, and leaving it at room temperature for 24 hours to form the lubricating coating.

[0020] In a fifth aspect, the present invention provides the application of the lubricating coating, or the lubricating coating obtained by the preparation method, or the lubricating coating, or the lubricating coating obtained by the preparation method in the lubrication treatment of friction pairs of large mechanical transmissions in low-orbit space.

[0021] In a sixth aspect, the present invention provides a lubrication treatment method for a friction pair of a large mechanical transmission in a space low-orbit orbit, comprising the following steps:

[0022] (1) sandblasting the surface of the large mechanical transmission friction pair with aluminum oxide sand;

[0023] (2) Use compressed air to blow the surface of the friction pair of large mechanical transmission after sandblasting;

[0024] (3) The lubricating coating according to claim 1 or 2 or the lubricating coating obtained by the preparation method according to claim 3 is sprayed on the surface of the friction pair of the large mechanical transmission after being purged by air pressure spraying.

[0025] Furthermore, in step (1), sandblasting is performed using 100 mesh alumina sand at a pressure of 0.3 MPa to 0.7 MPa.

[0026] Furthermore, in step (2), compressed air of 0.3 MPa to 0.5 MPa is used for purging.

[0027] Furthermore, in step (3), after spraying the lubricating coating, the coating is left at room temperature for 24 hours; the thickness of the lubricating coating formed by spraying the lubricating coating is 8 to 13 μm.

[0028] Furthermore, the large mechanical transmission friction pair for space low orbit is a large gear ring for space low orbit.

[0029] Furthermore, the friction pair of the space low-orbit large-scale mechanical transmission is made of stainless steel.

[0030] The technical solution of the present invention has the following advantages:

[0031] The lubricating coating provided by the present invention is composed of atomic oxygen-resistant sodium silicate as a binder, hyperbranched polysiloxane-modified molybdenum disulfide as a solid lubricant, antimony trioxide as a modifier, sodium fluorosilicate as a curing agent, and a dispersant and deionized water. On the one hand, the solid lubricant and the binder in the lubricating coating have good compatibility, and the prepared solid lubricating coating has a low vacuum friction coefficient, excellent wear resistance and load-bearing capacity, and excellent atomic oxygen resistance; on the other hand, the coating adopts a room temperature curing formula design, which can be sprayed on the surface of large movable parts, and is particularly suitable for lubrication and cold welding prevention of the surface of large mechanical transmission friction pairs affected by atomic oxygen in a low-orbit space environment. DETAILED DESCRIPTION

[0032] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0033] Sources of raw materials and instruments:

[0034] The chemical structural formula of the hyperbranched polysiloxane-modified molybdenum disulfide in the embodiment of the present invention is as follows:

[0035]

[0036] The preparation method of hyperbranched polysiloxane-modified molybdenum disulfide is as follows:

[0037] The silane coupling agent KH-580 and toluene were mixed and dissolved in a mass ratio of 1:10, and a silane coupling agent with a purity of ≥98% and D was added to the mixed solution in a mass ratio of KH-580 to molybdenum disulfide of 1:9. 50 The molybdenum disulfide powder of 1.5 μm was ultrasonically dispersed for 30 minutes, then heated to toluene reflux, stirred and kept warm for 10 hours. After the temperature was reduced to room temperature, molybdenum disulfide was centrifuged from the suspension by a high-speed centrifuge. The molybdenum disulfide powder was further washed with toluene and then centrifuged to obtain SH-MoS2 concentrated slurry. The prepared SH-MoS2 concentrated slurry was mixed according to the mass ratio of SH-MoS2 dry matter, isobutyltriethoxysilane, and neopentyl glycol of 14:6:3.3, and a 1:1 mixed solvent of toluene and N,N-dimethylformamide was added to start stirring, the material temperature was slowly increased to 100°C for insulation, and the distilled liquid was collected. Afterwards, while ensuring that the distillation temperature did not exceed 78°C, the material temperature was slowly and continuously increased to 160°C and kept warm for 5 hours. Cool down to room temperature and stop heating. Molybdenum disulfide was centrifuged from the suspension by a high-speed centrifuge. The molybdenum disulfide powder is further washed with toluene, and then centrifuged, and the washing and centrifugal separation processes are repeated three times. The powder is placed to dry at room temperature to obtain a hyperbranched polysiloxane-modified molybdenum disulfide powder.

[0038] Box sandblasting machine, Shanghai Liangshi Machinery Equipment Co., Ltd., LS9060A;

[0039] High-speed disperser, Zhangjiagang Tonghui Chemical Machinery Co., Ltd., SDF075;

[0040] Antimony trioxide, Hunan Anhua Huayu Antimony Industry Co., Ltd., particle size ≤ 0.5 μm;

[0041] SN5040, Japan Nopco SN-Dispersant-5040;

[0042] Sodium silicate, commercially available, modulus 3.1-3.4;

[0043] Sodium fluorosilicate, Yunnan Fluorine Environmental Protection Technology Co., Ltd., purity ≥99.0%.

[0044] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the art can be used. The raw materials or instruments used are all conventional products that can be obtained commercially, including but not limited to the raw materials or instruments used in the examples of this application.

[0045] Example 1

[0046] This embodiment provides a lubricating coating, which is composed of component A and component B.

[0047] Component A is composed of the following components: 50 parts of hyperbranched polysiloxane-modified molybdenum disulfide, 10 parts of antimony trioxide, 3 parts of SN5040, 11.4 parts of sodium fluorosilicate, and 223 parts of deionized water;

[0048] Component B is composed of the following components: 300 parts of sodium silicate and 200 parts of deionized water.

[0049] The preparation method of the lubricating coating is as follows:

[0050] The components in component A are mixed, dispersed at high speed and ground with zirconium oxide beads to obtain component A;

[0051] Mix and stir the components in component B to obtain component B;

[0052] Component A and component B are mixed and stirred evenly to obtain a lubricating coating.

[0053] Example 2

[0054] This embodiment provides a lubricating coating, which is composed of component A and component B.

[0055] Component A is composed of the following components: 150 parts of hyperbranched polysiloxane-modified molybdenum disulfide, 30 parts of antimony trioxide, 9 parts of SN5040, 3.8 parts of sodium fluorosilicate, and 668 parts of deionized water;

[0056] Component B is composed of the following components: 100 parts of sodium silicate and 66 parts of deionized water.

[0057] The preparation method of the lubricating coating is as described in Example 1.

[0058] Example 3

[0059] This embodiment provides a method for preparing a lubricating coating on a 9Cr18 steel test piece (Φ50 mm) and a large gear surface:

[0060] (1) The steel specimen and the tooth surface of the large gear were sandblasted with 100-mesh aluminum oxide sand at a pressure of 0.6 MPa using a box-type sandblasting machine;

[0061] (2) Use 0.3MPa compressed air to blow the sandblasted surface;

[0062] (3) The lubricating coating prepared in Example 1 was sprayed on the surface after the purging treatment by air pressure spraying, and left at room temperature for 24 hours to form a lubricating coating with a thickness of 10 μm.

[0063] Example 4

[0064] This embodiment provides a method for preparing a lubricating coating on a 9Cr18 steel specimen (Φ50 mm) and a large gear surface. The specific operation refers to that of Embodiment 3, except that the lubricating coating prepared in Embodiment 2 is sprayed on the surface after the purging treatment.

[0065] Experimental example

[0066] The large gear with lubricating coating prepared on the surface of Example 3 was subjected to a running life test. The contact stress during tooth meshing was 360 MPa. 6 After the grinding, the coating on the tooth surface was not worn through.

[0067] The 9Cr18 steel specimen with the lubricating coating prepared on the surface of Example 3 was subjected to a vacuum wear life test. The vacuum pressure was better than 1.3×10 -3 Pa vacuum atomic oxygen system, the coating was subjected to atomic oxygen action, and the atomic oxygen flux density used was (1±10%)×10 20 atom / m 2 ·s, the total accumulated atomic oxygen flux is 1.54×10 26 atoms / m 2 After the action, the vacuum wear life of the surface coating of the test ring was tested using a vacuum ball-on-disc friction tester, and the wear life was compared with that of the test ring that was not subjected to vacuum atomic oxygen action. The attenuation was no more than 20%.

[0068] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A lubricating coating, characterized in that: Including component A and component B, calculated by weight, The component A comprises: 50 to 150 parts of hyperbranched polysiloxane-modified molybdenum disulfide, 10 to 30 parts of antimony trioxide, 3 to 9 parts of a dispersant, 3.8 to 11.4 parts of sodium fluorosilicate, and 223 to 668 parts of deionized water; The component B comprises: 100 to 300 parts of sodium silicate and 66 to 200 parts of deionized water. The preparation method of the hyperbranched polysiloxane-modified molybdenum disulfide is as follows: 1) KH-580 and toluene are mixed to obtain a mixed solution, and then molybdenum disulfide powder is added to the mixed solution, ultrasonically dispersed uniformly, heated to toluene reflux, stirred and kept warm for more than 10 hours, cooled to room temperature after the insulation is completed, centrifuged, and the precipitate is washed with toluene to obtain SH-MoS2 concentrated slurry; 2) Mix the SH-MoS2 concentrated slurry, isobutyltriethoxysilane and neopentyl glycol, add them into a mixed solvent of toluene and N,N-dimethylformamide, stir and increase the material temperature to 100±5°C and keep it warm, and distill out the liquid; while ensuring that the distillation temperature does not exceed 78°C, continue to increase the material temperature to 160±5°C and keep it warm for more than 5 hours; after the insulation is completed, cool it to room temperature, centrifuge it, wash the precipitate with toluene, and dry it naturally to obtain a hyperbranched polysiloxane modified molybdenum disulfide powder.

2. The lubricating coating according to claim 1, characterized in that: The modulus of the sodium silicate is 3.1-3.4, and the solid content is 50%; In step 1), the total mass of the mixed solution is 100%, the mass fraction of KH-580 is 5% to 30%, and the mass fraction of toluene is 70% to 95%; the total mass of KH-580 and molybdenum disulfide powder is 100%, the mass fraction of KH-580 is 5% to 20%, and the mass fraction of molybdenum disulfide powder is 80% to 95%; the purity of the molybdenum disulfide powder is ≥98%, D 50 ≤1.5μm; In step 2), taking the total mass of dry matter SH-MoS2, isobutyltriethoxysilane and neopentyl glycol in the SH-MoS2 concentrated slurry as 100%, the mass fraction of dry matter SH-MoS2 is 50% to 70%, the mass fraction of isobutyltriethoxysilane is 20% to 30%, and the mass fraction of neopentyl glycol is 10% to 20%; in the mixed solvent of toluene and N,N-dimethylformamide, the volume ratio of toluene and N,N-dimethylformamide is 1:

1.

3. The method for preparing the lubricating coating according to claim 1 or 2, characterized in that: The following steps are involved: The hyperbranched polysiloxane-modified molybdenum disulfide, antimony trioxide, dispersant, sodium fluorosilicate and deionized water are mixed in proportion, and the mixture is subjected to high-speed dispersion and grinding with zirconium oxide beads to obtain component A; Mix sodium silicate and deionized water in proportion to obtain component B; The component A and the component B are mixed evenly to obtain the lubricating coating.

4. A lubricating coating, characterized in that: It is formed by the lubricating coating according to claim 1 or 2, or the lubricating coating obtained by the preparation method according to claim 3.

5. The method for preparing the lubricating coating according to claim 4, characterized in that: include: The lubricating coating is sprayed on the surface to be treated and left at room temperature for 24 hours to form the lubricating coating.

6. Use of the lubricating coating according to claim 1 or 2, or the lubricating coating obtained by the preparation method according to claim 3, or the lubricating coating according to claim 4, or the lubricating coating obtained by the preparation method according to claim 5 in the lubrication treatment of friction pairs of large-scale mechanical transmissions in low-orbit space.

7. A lubrication treatment method for a friction pair of a large mechanical transmission in a low-orbit space orbit, characterized in that: The following steps are involved: (1) sandblasting the surface of the large mechanical transmission friction pair with aluminum oxide sand; (2) Use compressed air to blow the surface of the friction pair of large mechanical transmission after sandblasting; (3) The lubricating coating according to claim 1 or 2 or the lubricating coating obtained by the preparation method according to claim 3 is sprayed on the surface of the friction pair of the large mechanical transmission after being purged by air pressure spraying.

8. The lubrication treatment method for the friction pair of a large space low-orbit mechanical transmission according to claim 7 is characterized in that: In step (1), 100 mesh alumina sand is used for sandblasting at a pressure of 0.3 MPa to 0.7 MPa; In step (2), purging is performed using compressed air of 0.3 MPa to 0.5 MPa; In step (3), after spraying the lubricating coating, the coating is left to stand at room temperature for 24 hours; the thickness of the lubricating coating formed by spraying the lubricating coating is 8 to 13 μm.

9. The lubrication treatment method for the friction pair of a large space low-orbit mechanical transmission according to claim 7 is characterized in that: The large mechanical transmission friction pair for space low orbit is a large gear ring for space low orbit.

10. The lubrication treatment method for the friction pair of a large space low-orbit mechanical transmission according to claim 7, characterized in that: The friction pair of the space low-orbit large-scale mechanical transmission is made of stainless steel.

Citation Information

Patent Citations

  • Aqueous environment-friendly inorganic high-temperature-resistant self-lubricating paint as well as preparation method and application thereof

    CN106810916A