A high-purity alumina active spherical carrier and preparation method thereof

Through the high-purity alumina active sphere support catalyst, the problems of high catalyst cost and low yield in the production of icimerin are solved, and the high yield and low cost production of compound B is achieved, which is suitable for large-scale industrial applications.

CN116673067BActive Publication Date: 2024-12-06YANGZHOU ZHONGTIANLI NEW MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310491738.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-12-06
Estimated Expiration
2043-05-05

AI Technical Summary

Technical Problem

In the production process of icimerin in the prior art, the catalyst cost is high and the yield is low, making it difficult to meet the needs of large-scale industrial production.

Method used

Using high-purity alumina active sphere carrier, it is prepared by immersion, drying, calcining and pressurization treatment, and is used as catalysts to promote the weight of compound A. The reaction of the displacement produces compound B.

Benefits of technology

It improves the yield of compound B, reduces production costs, is convenient to operate, is suitable for large-scale production, has sufficient raw materials, and is suitable for cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the technical field of alumina carriers, and more particularly to a high-purity alumina active ball carrier and a preparation method thereof. The catalyst is prepared from the following raw materials in parts by weight: 30 to 40 parts of ZSM-48 molecular sieves, 45 to 60 parts of lanthanide metal nitrate solutions, and 15 to 20 parts of high-purity alumina. The present invention uses a ZSM-48 molecular sieve modified by ytterbium nitrate solution, and combines the carrier prepared by high-purity alumina active balls. When used as a catalyst, it effectively promotes the rearrangement reaction of compound A to generate compound B, improves the yield of compound B, thereby expanding the source of icariin intermediates and reducing the production and preparation cost of icariin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alumina carriers, and in particular to a high-purity alumina active spherical carrier and a preparation method thereof. Background Art

[0002] Icariin, also known as icariin and icariin, is a new effective monomer obtained by enzymatic conversion of icariin, the main active ingredient extracted and separated from the traditional Chinese medicine Epimedium. The preparation method of the compound is disclosed in CN101302548B. The method uses icariin as a raw material, hydrolyzes it with β-glucosidase, dissolves the precipitate obtained by centrifugation of the hydrolyzate with acetone, and centrifuges to obtain a supernatant. The supernatant obtained by centrifugation is then recrystallized with water to obtain pure icariin.

[0003] In the March 2013 issue of Organic Chemistry, an article entitled "Synthesis of Icariin" was published. The synthetic route in the article is the same as that of 200610165354.7. However, in the rearrangement process from compound (12) to compound (13), tris(6,6,7,7,8,8,8-heptafluoro-2,2-dimethyl-3,5-octanedione)europium was used as a catalyst. The reaction temperature during the catalytic process reached 80°C, the reaction time was 36 hours, and the yield was only 42%. In order to obtain a higher purity compound 12 for the next reaction, the article separated compound (12) by column chromatography on a silica gel column. Although the above separation is feasible in the laboratory, it is too costly and not suitable for large-scale industrial production.

[0004] CN201710565818.1 discloses a method for synthesizing icariin, which involves the synthesis of an icariin intermediate, as shown below:

[0005]

[0006] However, the yield of the target intermediate of this synthesis method is low, less than 50%, and the cost is high, which cannot meet the needs of large-scale production.

[0007] Based on the above situation, the present invention proposes a high-purity alumina active spherical carrier and a preparation method thereof, which can effectively solve the above problems as a catalyst in the above process. Summary of the invention

[0008] The object of the present invention is to provide a high-purity alumina active spherical carrier and a preparation method thereof.

[0009] To achieve the above object, the present invention provides a high-purity alumina active spherical carrier, which is prepared from the following raw materials in parts by weight: 30 to 40 parts of ZSM-48 molecular sieve, 45 to 60 parts of nitrate solution of lanthanide metals, and 15 to 20 parts of high-purity alumina.

[0010] Preferably, the silicon to aluminum molar ratio of the ZSM-48 molecular sieve is 56-64.

[0011] Preferably, the lanthanide metal nitrate solution includes one of ytterbium nitrate solution, europium nitrate solution, cerium nitrate solution and praseodymium nitrate solution.

[0012] Preferably, the lanthanide metal nitrate solution is ytterbium nitrate solution.

[0013] Preferably, the concentration of the ytterbium nitrate solution is 0.1-0.3 g of ytterbium nitrate per milliliter of aqueous solution.

[0014] Preferably, the purity of the high-purity alumina is 99.9% and the specific surface area is 100-130m 2 / g, and the average particle size is 200~250nm.

[0015] The present invention also provides a method for preparing a high-purity alumina active spherical carrier, the method comprising the following steps:

[0016] (1) adding ZSM-48 molecular sieve to ytterbium nitrate solution, impregnating at room temperature for 12-13 hours, filtering, collecting solid particles, and drying at 150°C for 2-3 hours to obtain a precursor;

[0017] (2) mixing the precursor obtained in step (1) with high-purity alumina, stirring the mixture at 100-150 rpm for 30-45 min to make it uniform, and then calcining at 300-350° C. for 8-10 h to obtain an inactivated carrier;

[0018] (3) The carrier obtained in step (3) is placed in a pressurized environment filled with inert gas for 10 to 12 hours, wherein the pressurized environment is 1.5 to 2 MPa, thereby obtaining the high-purity alumina active sphere carrier.

[0019] Preferably, the inert gas is one of nitrogen, carbon dioxide, argon and helium.

[0020] The present invention also provides a use of a high-purity alumina active spherical carrier, which is used as a catalyst in the process of synthesizing compound B from compound A:

[0021] The method for synthesizing compound B from compound A is as follows: under nitrogen protection, compound A, solvent toluene, and high-purity alumina active ball carrier are sequentially added into a reaction container; the reaction solution is heated to 80-90° C. and stirred for 18 hours; the reaction solution is cooled to room temperature, filtered, and the filter cake is sequentially washed with dichloromethane and acetonitrile; filtered, and dried to obtain compound B.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The ZSM-48 molecular sieve modified by ytterbium nitrate solution in the present invention is combined with a carrier prepared by high-purity alumina active balls. When used as a catalyst, it effectively promotes the rearrangement reaction of compound A to generate compound B, improves the yield of compound B, thereby expanding the source of icariin intermediates and reducing the production and preparation cost of icariin.

[0024] 2. The preparation method of the present invention is easy to operate, easy to mass produce, and has stable quality.

[0025] 3. The raw materials of the present invention are sufficient in the country and are of suitable price, so that there is no high cost restriction for large-scale production. DETAILED DESCRIPTION

[0026] Example 1

[0027] The amount of each raw material is shown in Table 1.

[0028] (1) adding ZSM-48 molecular sieve into ytterbium nitrate solution, impregnating at room temperature for 12 hours, filtering, collecting solid particles, and drying at 150°C for 2 hours to obtain a precursor;

[0029] (2) mixing the precursor obtained in step (1) with high-purity alumina, stirring the mixture at 100 rpm for 45 min to make it uniform, and then calcining at 300° C. for 10 h to obtain an unactivated carrier;

[0030] (3) The carrier obtained in step (3) is placed in a pressurized environment filled with inert gas for 12 hours, wherein the pressurized environment is 1.5 MPa, to obtain a high-purity alumina active sphere carrier.

[0031] Example 2

[0032] The amount of each raw material is shown in Table 1.

[0033] (1) adding ZSM-48 molecular sieve into ytterbium nitrate solution, impregnating at room temperature for 13 hours, filtering, collecting solid particles, and drying at 150°C for 3 hours to obtain a precursor;

[0034] (2) mixing the precursor obtained in step (1) with high-purity alumina, stirring the mixture at 150 rpm for 30 min to make it uniform, and then calcining at 350° C. for 8 h to obtain an unactivated carrier;

[0035] (3) The carrier obtained in step (3) is placed in a pressurized environment filled with inert gas and treated for 10 hours, wherein the pressurized environment is 2 MPa, to obtain a high-purity alumina active sphere carrier.

[0036] Example 3

[0037] The amount of each raw material is shown in Table 1.

[0038] (1) adding ZSM-48 molecular sieve into ytterbium nitrate solution, impregnating at room temperature for 13 hours, filtering, collecting solid particles, and drying at 150°C for 3 hours to obtain a precursor;

[0039] (2) mixing the precursor obtained in step (1) with high-purity alumina, stirring the mixture at 150 rpm for 45 min to make it uniform, and then calcining at 350° C. for 10 h to obtain an unactivated carrier;

[0040] (3) The carrier obtained in step (3) is placed in a pressurized environment filled with inert gas and treated for 12 hours, wherein the pressurized environment is 2 MPa, to obtain a high-purity alumina active sphere carrier.

[0041] Comparative Example 1

[0042] The amount of each raw material is shown in Table 1.

[0043] (1) adding ZSM-5 molecular sieve into ytterbium nitrate solution, impregnating at room temperature for 13 hours, filtering, collecting solid particles, and drying at 150°C for 3 hours to obtain a precursor;

[0044] (2) mixing the precursor obtained in step (1) with high-purity alumina, stirring the mixture at 150 rpm for 45 min to make it uniform, and then calcining at 350° C. for 10 h to obtain an unactivated carrier;

[0045] (3) The carrier obtained in step (3) is placed in a pressurized environment filled with inert gas and treated for 12 hours, wherein the pressurized environment is 2 MPa, to obtain a high-purity alumina active sphere carrier.

[0046] Comparative Example 2

[0047] The amount of each raw material is shown in Table 1.

[0048] (1) adding ZSM-22 molecular sieve into ytterbium nitrate solution, impregnating at room temperature for 13 hours, filtering, collecting solid particles, and drying at 150°C for 3 hours to obtain a precursor;

[0049] (2) mixing the precursor obtained in step (1) with high-purity alumina, stirring the mixture at 150 rpm for 45 min to make it uniform, and then calcining at 350° C. for 10 h to obtain an unactivated carrier;

[0050] (3) The carrier obtained in step (3) is placed in a pressurized environment filled with inert gas and treated for 12 hours, wherein the pressurized environment is 2 MPa, to obtain a high-purity alumina active sphere carrier.

[0051] Comparative Example 3

[0052] The amount of each raw material is shown in Table 1.

[0053] (1) adding ZSM-48 molecular sieve to ytterbium trifluoromethanesulfonate solution, impregnating at room temperature for 13 h, filtering, collecting solid particles, and drying at 150 ° C for 3 h to obtain a precursor;

[0054] (2) mixing the precursor obtained in step (1) with high-purity alumina, stirring the mixture at 150 rpm for 45 min to make it uniform, and then calcining at 350° C. for 10 h to obtain an unactivated carrier;

[0055] (3) The carrier obtained in step (3) is placed in a pressurized environment filled with inert gas and treated for 12 hours, wherein the pressurized environment is 2 MPa, to obtain a high-purity alumina active sphere carrier.

[0056] Comparative Example 4

[0057] The amount of each raw material is shown in Table 1.

[0058] (1) adding ZSM-48 molecular sieve into ytterbium nitrate solution, impregnating at room temperature for 13 hours, filtering, collecting solid particles, and drying at 150°C for 3 hours to obtain a precursor;

[0059] (2) The precursor obtained in step (3) is placed in a pressurized environment filled with inert gas and treated for 12 hours, wherein the pressurized environment is 2 MPa, to obtain a carrier.

[0060] Comparative Example 5

[0061] The amount of each raw material is shown in Table 1.

[0062] (1) adding ZSM-48 molecular sieve into ytterbium nitrate solution, impregnating at room temperature for 13 hours, filtering, collecting solid particles, and drying at 150°C for 3 hours to obtain a precursor;

[0063] (2) The precursor obtained in step (1) was mixed with high-purity alumina, stirred at 150 rpm for 45 min to make it uniform, and then calcined at 350° C. for 10 h to obtain a high-purity alumina active sphere carrier.

[0064] Table 1

[0065]

[0066] Catalyst performance evaluation test

[0067] The high-purity alumina active sphere carrier prepared in Examples 1 to 3 and Comparative Examples 1 to 5 was crushed and sieved to a particle size of 20 to 30 meshes. Under nitrogen protection, compound A (50 g, 0.11 mol), toluene (500 mL, 10 mL / g) (solvent) were added to the reaction bottle, and the above catalyst (25 g) was taken. The reaction solution was heated to 80 to 90 ° C and stirred for 18 hours; the reaction solution was cooled to room temperature, filtered, and the filter cake was washed with dichloromethane (200 mL, 4 mL / g). The filtrate was combined and concentrated to 100 mL. Acetonitrile (250 mL, 5 mL / g) was added to the concentrated solution and concentrated to 100 mL. Acetonitrile (250 mL, 5 mL / g) was added again and concentrated to 250 mL. After stirring at 50-60°C for 1 hour, the temperature was lowered to 0°C within 2 hours and stirred for 1 hour; the filter cake was washed with acetonitrile (50 mL, 1 mL / g) and dried to obtain compound B; the yield of compound B was calculated. The results are shown in Table 2.

[0068] Table 2 Reaction results

[0069]

[0070] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. A use of a high-purity alumina active ball carrier, characterized in that: The use is to use compound A as a catalyst in the process of synthesizing compound B: ; The high-purity alumina active sphere carrier is prepared from the following raw materials in parts by weight: 30-40 parts of ZSM-48 molecular sieve, 45-60 parts of nitrate solution of lanthanide metals, and 15-20 parts of high-purity alumina.

2. The use according to claim 1, characterized in that The method for synthesizing compound B from compound A is as follows: under nitrogen protection, compound A, solvent toluene, and high-purity alumina active ball carrier catalyst are sequentially added into a reaction container; the reaction liquid is heated to 80-90° C. and stirred for 18 hours; the reaction liquid is cooled to room temperature, filtered, and the filter cake is sequentially washed with dichloromethane and acetonitrile; filtered, and dried to obtain compound B.

3. The use according to claim 1, characterized in that The silicon-aluminum molar ratio of the ZSM-48 molecular sieve is 56-64.

4. The use according to claim 1, characterized in that The lanthanide metal nitrate solution includes one of ytterbium nitrate solution, europium nitrate solution, cerium nitrate solution and praseodymium nitrate solution.

5. The use according to claim 4, characterized in that The lanthanide metal nitrate solution is ytterbium nitrate solution.

6. The use according to claim 3, characterized in that: The concentration of the ytterbium nitrate solution is 0.1-0.3 g of ytterbium nitrate per milliliter of aqueous solution.

7. The use according to claim 1, characterized in that The purity of the high-purity alumina is 99.9% and the specific surface area is 100-130m 2 / g, and the average particle size is 200~250nm.

8. The use according to claim 1, characterized in that The preparation method of the high-purity alumina active sphere carrier comprises the following steps: (1) Adding ZSM-48 molecular sieve to ytterbium nitrate solution, impregnating at room temperature for 12-13 hours, filtering, collecting solid particles, and drying at 150°C for 2-3 hours to obtain a precursor; (2) mixing the precursor obtained in step (1) with high-purity alumina, stirring the mixture at 100-150 rpm for 30-45 min to make it uniform, and then calcining at 300-350° C. for 8-10 h to obtain a carrier; (3) The carrier obtained in step (3) is placed in a pressurized environment filled with inert gas and treated for 10 to 12 hours, wherein the pressurized environment is 1.5 to 2 MPa, to obtain a supported catalyst.

9. The use according to claim 8, characterized in that The inert gas is one of nitrogen, carbon dioxide, argon and helium.