A method for preparing a rare earth substituted multiferroic M-type strontium lanthanum ferrite material
The multiferroic M-type strontium lanthanum ferrite material substituted by rare earth solves the problems of insufficient application of antiferroelectric materials and poor performance in high temperature environments in the existing technology, and achieves high energy storage efficiency and magnetic semiconductor properties. Ceramic material preparation provides greater application possibilities for energy storage devices and memory devices.
Patent Information
- Application Number
- CN202310115829.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-15
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-02-15
AI Technical Summary
In the existing technology, capacitors made of non-magnetic antiferroelectric materials have poor application prospects in energy storage devices and memory devices, and traditional inorganic dielectric capacitors have poor performance in high-temperature environments and cannot meet the requirements of multi-function, low power consumption and environmental protection. Equipment needs.
Using rare earth-substituted multiferroic M-type strontium lanthanum ferrite material, LaxSr1-xFe12O19 nanopowder is prepared by replacing Sr ions in SrFe12O19 with La ions, forming a new ceramic material with improved energy storage efficiency and magnetic properties. Semiconductor properties, magnetocapacitance effect and giant magnetoresistance effect.
The energy storage efficiency is significantly improved, and the real and imaginary parts of the dielectric constant and complex impedance are enhanced, providing greater possibilities for the development of new energy storage devices and memory devices.
Smart Images

Figure CN116675526B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of energy storage device ceramic material preparation, and in particular to a preparation method of a rare earth substituted multiferroic M-type strontium lanthanum ferrite material. Background Art
[0002] In the era of rapid development of artificial intelligence and information technology, the pursuit of miniaturization of storage devices, consumer electronics and energy-saving devices has inspired people to explore new multifunctional materials to replace semiconductor technology. Among a large number of advanced technology materials, multiferroic materials show excellent physical properties and unique technological applications. Multiferroic materials represent a new type of material in which multiple ferroic properties coexist in an orderly manner. Their coupling can produce additional ordering parameters. Therefore, these can form new multifunctional devices and are widely used in multifunctional, low-power, environmentally friendly and other devices.
[0003] As an energy storage device, dielectric capacitors are widely used. Organic dielectric capacitors can withstand very high electric field strength to produce high energy storage density, but they have a low melting point and melt due to heat generation after rapid back and forth charging and discharging, which makes them only suitable for low temperature environments; inorganic dielectric capacitors, mainly traditional perovskite compounds, not only have relatively high energy density, but can also continue to work at higher temperatures without affecting performance. Compared with organic dielectrics, inorganic dielectrics have a wider range of applications and simpler conditions of use.
[0004] Antiferroelectric (AFE) materials have higher energy storage density than ferroelectric (FE) materials because they have extremely low remnant polarization and double hysteresis loops, which makes them have greater application prospects than ferroelectric materials. As for capacitors made of non-magnetic antiferroelectric materials, they can only be charged in one-dimensional electric field and have poor application prospects in energy storage devices and memory devices. Therefore, the present invention proposes a method for preparing a rare earth substituted multiferroic M-type strontium lanthanum ferrite material to solve the problems existing in the prior art. Summary of the invention
[0005] In view of the above problems, the present invention aims to provide a method for preparing a rare earth substituted multiferroic M-type strontium lanthanum ferrite material, wherein the method for preparing the rare earth substituted multiferroic M-type strontium lanthanum ferrite material is to replace SrFe with La ions. 12 O 19 La formed by Sr ions in x Sr 1-x Fe 12 O 19Nanopowders are used to prepare a new type of ceramic material, which has greatly improved energy storage efficiency and has the characteristics of magnetic semiconductors. It also has magnetocapacitive effect and giant magnetoresistance effect. Both the real and imaginary parts of the dielectric constant and complex impedance are improved, providing greater possibilities for the development of new energy storage devices and memory devices.
[0006] To achieve the purpose of the present invention, the present invention is implemented by the following technical scheme: a method for preparing a rare earth substituted multiferroic M-type strontium lanthanum ferrite material, comprising the following steps:
[0007] Step 1: Preparation of a first precursor: weigh 6 g of ferric acetylacetonate and dissolve it in 100 ml of acetone solvent, then pour it into a three-necked flask, and stir it at 70° C. for 6 hours in a glove box using a heating coil to obtain a first precursor;
[0008] Step 2, preparation of the second precursor, weigh lanthanum acetate and strontium acetate according to the La: Sr: Fe molar ratio of 0.6: 0.4: 10, and then pour them into a single-necked flask filled with 15 ml of glycerol to dissolve and mix, and then distill the mixed solution in a rotary evaporator at 120 ° C for 2 hours, and transfer it to a 20 ml volumetric flask after it is completely dissolved, so as to obtain the second precursor;
[0009] Step 3: Precursor mixing reaction: pour the second precursor into the three-necked flask containing the first precursor in the glove box in step 1, stir at 70°C for 6 hours, then add 60 ml of ammonia water to the precursor mixture, and react at 70°C for 24 hours to obtain a solution with particle precipitate;
[0010] Step 4: After the precipitation is extracted, the three-necked flask with the precipitation is transferred to a centrifuge and centrifuged at 10,000 rpm for 15 minutes to remove the organic solvent to obtain precipitation particles, which are then calcined and ground twice to obtain single-phase hexaferrite La 0.6 Sr 0.4 Fe 12 O 19 Nano powder;
[0011] Step 5: Sample preparation and testing: Weigh 0.06 g of single-phase hexaferrite nanopowder, press it into particles, and then sinter and anneal it to make a ceramic sample. Then use instruments to test the performance of the ceramic sample and record the test results.
[0012] A further improvement is that when the distilled solution is transferred to a 20 ml volumetric flask in step 2, the small amount of solution remaining in the single-necked flask is rinsed with alcohol and poured into the volumetric flask; when the second precursor is poured into the three-necked flask in step 3, the small amount of solution remaining in the volumetric flask is also rinsed with alcohol and poured into the three-necked flask.
[0013] A further improvement is that the two calcination treatments in step 4 are respectively calcined at 450°C for 1 hour and then ground for 30 minutes, then calcined at 800°C for 1 hour and then ground for 30 minutes, and then calcined at 750°C under oxygen conditions for 3 hours to remove organic impurities and nano-grind to obtain single-phase hexaferrite.
[0014] A further improvement is that the specific preparation method of the ceramic pattern in step 5 includes
[0015] S1. Weigh 0.06 g of single-phase hexaferrite nanopowder, press it into particles in a module and sinter it at 1350°C for 2 h to obtain a solid sample;
[0016] S2, annealing the solid sample in a tube furnace at 800°C in a pure oxygen environment for 6 hours, then turning it over and continuing annealing for 6 hours, and then heat treating it in a high-temperature oxygen environment at 750°C for 3 hours to obtain a ceramic sample semi-finished product;
[0017] S3. Silver paste is applied on both sides of the semi-finished ceramic pattern and cured at 820° C. for 15 minutes to form silver electrodes, thereby obtaining a finished ceramic pattern.
[0018] A further improvement is that the instruments for detecting the performance of the ceramic sample in the step five include an X-ray diffractometer for identifying the structure of the sample, a vibrating sample magnetometer for detecting the magnetic properties of the sample, an ultraviolet-visible-near-infrared spectrophotometer for testing the optical properties of the sample, a ZT-IA ferroelectric tester for measuring the PE hysteresis loop of the sample, a Hioki IM3533-01 LCR meter for measuring the dielectric spectrum and impedance spectrum, a Keithley 2450 source meter for recording the giant magnetoresistance effect, and a Microtest Precision 6630 LCR meter for recording the magneto-dielectric response.
[0019] The beneficial effects of the present invention are as follows: the present invention replaces SrFe with La ions 12 O 19 La formed by Sr ions in x Sr 1-x Fe 12 O 19 Nanopowders are used to prepare a new type of ceramic material, which has greatly improved energy storage efficiency and has the characteristics of magnetic semiconductors. It also has magnetocapacitive effect and giant magnetoresistance effect. Both the real and imaginary parts of the dielectric constant and complex impedance are improved, providing greater possibilities for the development of new energy storage devices and memory devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a flow chart of the method of Example 1 of the present invention.
[0021] Figure 2 This is a flow chart of the ceramic pattern preparation method according to Example 1 of the present invention.
[0022] Figure 3 is La in Example 2 of the present invention 0.6 Sr 0.4 Fe 12 O 19 X-ray diffraction (XRD) patterns of the compounds.
[0023] Figure 4 This is the fully saturated double PE hysteresis loop diagram of L6S4FO in Example 2 of the present invention.
[0024] Figure 5 This is a curve diagram of the change in energy density-electric field (WE) of the L6S4FO ceramic sample in Example 2 of the present invention.
[0025] Figure 6 1 is a paraelectric hysteresis loop diagram of L7S3FO at different voltages in Example 2 of the present invention.
[0026] Figure 7 1 and 2 are hysteresis loop diagrams of L6S4FO tested after calcination and annealing at 1350°C (a) and 1400°C (b) in Example 2 of the present invention.
[0027] Figure 8 2 are the hysteresis loop diagrams of L7S3FO (a) and L6S4FO (b) after annealing at 1400°C in Example 2 of the present invention.
[0028] Fig. 9 Graph showing the absorption spectra of L6S4FO and L7S3FO and the function of photon energy E in Example 2 of the present invention.
[0029] Fig.10 This is a function diagram of the relationship between the real part of the dielectric constant and the magnetic field at three frequencies in Example 2 of the present invention.
[0030] Fig.11 1 is a function diagram of the relationship between complex impedance and frequency under different magnetic fields (B) of Example 2 of the present invention.
[0031] Fig.12 This is a simplified equivalent circuit model diagram of the capacitor according to Example 2 of the present invention.
[0032] Fig.13 1 is a function diagram showing the relationship between MR{(ZB-Z0) / ZB}(%) and frequency under different magnetic fields (B) in Example 2 of the present invention.
[0033] Fig.14 Graph showing the relationship between the real part (Z') and the imaginary part (Z") of the complex impedance under different magnetic fields (B) in Example 2 of the present invention. DETAILED DESCRIPTION
[0034] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.
[0035] Example 1
[0036] according to Figure 1 and Figure 2 As shown, this embodiment provides a method for preparing a rare earth substituted multiferroic M-type strontium lanthanum ferrite material, comprising the following steps:
[0037] Step 1: Preparation of a first precursor: weigh 6 g of ferric acetylacetonate and dissolve it in 100 ml of acetone solvent, then pour it into a 250 ml three-necked flask, and stir it at 70 ° C. in a glove box using a heating coil for 6 hours to obtain a first precursor;
[0038] Step 2, preparation of the second precursor, weigh lanthanum acetate and strontium acetate according to the La: Sr: Fe molar ratio of 0.6: 0.4: 10, and then pour them into a single-necked flask filled with 15 ml of glycerol to dissolve and mix, and then distill the mixed solution in a rotary evaporator at 120 ° C for 2 hours to prevent the influence of water molecules in the air on the material; after the lanthanum acetate and strontium acetate are completely dissolved, transfer them to a 20 ml volumetric flask, and during the transfer, rinse the small amount of solution remaining in the single-necked flask with alcohol and pour it into the volumetric flask together to obtain the second precursor;
[0039] Step 3: Precursor mixing reaction: pour the second precursor into the three-necked flask containing the first precursor in the glove box in step 1, then rinse the small amount of solution remaining in the volumetric flask with alcohol and pour it into the three-necked flask to mix the second precursor and the first precursor, stir at 70°C for 6h, then add 60ml of ammonia water to the precursor mixture, and react at 70°C for 24h to ensure that all La, Sr, and Fe ions are precipitated to obtain a solution with a granular precipitate;
[0040] Step 4: After the precipitation is extracted, the three-necked flask with the precipitation is transferred to a centrifuge and centrifuged at 10,000 rpm for 15 minutes to remove the organic solvent to obtain precipitation particles, which are then calcined and ground twice to obtain single-phase hexaferrite La 0.6 Sr 0.4 Fe 12 O 19 Nano powder;
[0041] The two calcination treatments were calcination at 450°C for 1 hour and then grinding for 30 minutes, then calcination at 800°C for 1 hour and then grinding for 30 minutes, and then calcination at 750°C for 3 hours under oxygen conditions to remove organic impurities and nano-grinding to obtain single-phase hexaferrite.
[0042] Step 5: Sample preparation and testing: weigh 0.06 g of single-phase hexaferrite nanopowder, press it into particles, sinter and anneal it to make a ceramic sample, and then use instruments to test the performance of the ceramic sample and record the test results;
[0043] The specific preparation method of the ceramic pattern includes:
[0044] S1. Weigh 0.06 g of single-phase hexaferrite nanopowder, press it into particles in a module and sinter it at 1350°C for 2 h to obtain a solid sample;
[0045] S2, annealing the solid sample in a tube furnace at 800°C in a pure oxygen environment for 6 hours, then turning the solid sample over and continuing to anneal at the same temperature for 6 hours, and then heat treating it in a high-temperature oxygen environment at 750°C for 3 hours to remove oxygen vacancies and convert Fe2+ into Fe3+ as much as possible, thereby greatly improving the resistance of the ceramic and reducing leakage in subsequent ferroelectric measurements, thus obtaining a ceramic sample semi-finished product;
[0046] S3. Silver paste is applied on both sides of the semi-finished ceramic pattern and cured at 820° C. for 15 minutes to form silver electrodes, thereby obtaining a finished ceramic pattern.
[0047] The instruments used to test the performance of ceramic samples include an X-ray diffractometer for identifying the structure of the samples, a vibrating sample magnetometer for testing the magnetic properties of the samples, a UV-visible-near-infrared spectrophotometer for testing the optical properties of the samples, a ZT-IA ferroelectric tester for measuring the PE hysteresis loop of the samples, a Hioki IM 3533-01LCR meter for measuring the dielectric spectrum and impedance spectrum, a Keithley 2450 source meter for recording the giant magnetoresistance effect, and a Microtest Precision 6630 LCR meter for recording the magneto-dielectric response.
[0048] Example 2
[0049] according to Figure 3-Figure 14 As shown, this embodiment is a method for preparing a rare earth substituted multiferroic M-type strontium lanthanum ferrite material in Example 1, and the single-phase hexaferrite La 0.6 Sr 0.4 Fe 12 O 19 Performance test results of nanopowders and ceramic samples made from them.
[0050] Another group of single-phase hexaferrite La was prepared by changing the content of substituted lanthanum ions using the preparation method in Example 1. 0.7 Sr 0.3 Fe 12 O 19 Nanopowder, both are expressed as single-phase La x Sr 1-x Fe 12 O 19 (x=0.6 or 0.7).
[0051] 1. La x Sr 1-x Fe 12 O 19 Structural analysis of compounds (x = 0.6 or 0.7)
[0052] Referring to the ceramic sample preparation of step 5 of Example 1, the powder was placed in a mold and pressed into a sheet form, and then sintered into ceramics at 1350°C and 1400°C respectively. After sintering, the ceramic was heat treated three times in O2 to remove oxygen vacancies and x Sr 1-x Fe 12 O 19 (x=0.6 or 0.7) 2+ Fully converted into Fe 3+ As the instruction manual Figure 3 As shown, the diffraction peak above shows La 0.6 Sr 0.4 Fe 12 O 19 X-ray diffraction (XRD) spectrum of the compound. The diffraction peak close to the horizontal axis at the bottom is SrFe 12 O 19 The standard diffraction spectrum of La 0.6 Sr 0.4 Fe 12 O 19 All diffraction peaks of pure SrFe 12 O 19 The diffraction peaks in the standard card match well, there is no second phase ferrite or other oxide impurities, and the peaks of each diffraction peak are sharp, indicating that the crystallization is complete. 0.7 Sr 0.3 Fe 12 O 19 The diffraction peaks of La 0.7 Sr 0.3 Fe 12 O 19 It is completely consistent, except that with the increase of substitution, the diffraction peak has a certain orientation as shown in the attached manual. Figure 3The inset shows the trend of the right shift. In summary, it shows that these two different ratios of La replacing SrFe 12 O 19 La x Sr 1-x Fe 12 O 19 (x=0.6 or 0.7) The compound was successfully prepared.
[0053] Instructions attached Figure 3 Figure illustration (a) Standard SrFe 12 O 19 (b) La 0.6 Sr 0.4 Fe 12 O 19 、(c)La 0.7 Sr 0.3 Fe 12 O 19 The diffraction peak of the (110) lattice plane.
[0054] 2.La x Sr 1-x Fe 12 O 19 (x=0.6 or 0.7) Analysis of the transition from ferroelectricity to antiferroelectricity and then to paraelectricity
[0055] SrFe 12 O 19 Expressed in SFO, La 0.6 Sr 0.4 Fe 12 O 19 Expressed as L6S4FO, La 0.7 Sr 0.3 Fe 12 O 19 Indicated by L7S3FO, as shown in the instruction manual Figure 4 As shown, the fully saturated double PE hysteresis loop of L6S4FO is shown, proving the intrinsic antiferroelectricity of L6S4FO. When the applied electric field is less than 300KV / cm, the net macroscopic remnant polarization is almost zero, and the maximum does not exceed 1.7uC / cm 2 . When the external electric field continues to increase, the PE loop shows an obvious double hysteresis loop in the high electric field region, showing the characteristics of nonlinear polarization. These perfectly match the two characteristics of the antiferroelectric PE hysteresis loop. The forward phase switching field (EF) from antiferroelectric to ferroelectric and the reverse switching field (EA) from ferroelectric to antiferroelectric can be estimated by the intersection of the steepest part of the hysteresis loop and the electric field axis. Figure 4It can be seen that when the external electric field is greater than 483KV / cm (EF), the polarization intensity increases sharply with the increase of the electric field. Under this electric field, the antiparallel dipoles in the crystal begin to rotate to the same direction, and the antiferroelectric phase is induced to the ferroelectric phase. When the external electric field reaches 583KV / cm, the polarization intensity reaches saturation, and the saturated polarization intensity is 58.884uC / cm 2 When the external electric field is less than 443KV / cm (EA), the metastable ferroelectric phase is induced to return to the original antiferroelectric phase, that is, the dipoles return to the original antiparallel arrangement. Similarly, these two transitions also exist when a reverse voltage is applied.
[0056] The energy density of an antiferroelectric can be calculated using the following formula:
[0057]
[0058] Calculated Instructions Attached Figure 4 The AFE double PE hysteresis loop shows that the energy density of L6S4FO is 26.36 J / cm 3 , the energy storage efficiency is as high as 76.75%. Its energy density and energy storage efficiency are higher than those of multilayer film (Pb 0.92 2La 0.08 )(Zr 0.65 Ti 0.35 Zr0.65Ti0.35)O3 / PbZrO3.
[0059] As the instruction manual Figure 5 As shown, it shows the energy density-electric field (WE) curve. When the voltage is less than 300KV / cm, the energy density (W) increases slowly with the increase of the electric field (E). When the voltage is greater than 300KV / cm, the energy density (W) increases sharply with the increase of the electric field (E). Figure 5 The AFE double PE hysteresis loop is tested for different L6S4FO ceramic samples. Testing different samples proves its repeatability and reliability. The energy density is 31.35J / cm 3 The energy storage efficiency is as high as 88.64%. The energy density under each electric field of the curve is shown in the attached manual. Figure 5 The double PE hysteresis loop is calculated by the energy density formula of antiferroelectrics. Figure 5 The inset in Figure 2 shows the AFEP-E hysteresis loop of another L6S4FO ceramic sample, demonstrating the repeatability and reliability of the experiment.
[0060] As the instruction manual Figure 6 As shown, the paraelectric hysteresis loop of L7S3FO at different voltages is shown. It can be seen that the polarization intensity increases steadily and linearly with the increase of voltage, showing obvious paraelectricity (abbreviated as PE). Figure 6 The maximum applied voltage and polarization intensity show an obvious linear relationship, which further confirms the PE of L7S3FO. In summary, the antiferroelectricity of L6S4FO and the paraelectricity of L7S3FO at room temperature are proved. It is also proved that by increasing the amount of strontium ions in SFO replaced by lanthanum ions, the original ferroelectricity (SFO) can be converted to antiferroelectricity (L6S4FO) and then to paraelectricity (L7S3FO).
[0061] 3. La x Sr 1-x Fe 12 O 19 Analysis of magnetic semiconductor properties of (x=0.6 or 0.7) compounds
[0062] The magnetic properties of L6S4FO and L7S3FO powder samples were tested using a vibrating sample magnetometer (VSM). Figure 7 The hysteresis loops shown are those obtained by testing L6S4FO after calcining at 1350℃ (a) and 1400℃ (b) for 2h, and then annealing in an O2 environment at 800℃ for 6h. The saturation magnetization (Ms) of the sample calcined at 1350℃ is 41.941emu / g, and the coercive field (Hc) is about 2281.3Oe. The saturation magnetization (Ms) of the sample calcined at 1400℃ is 58.866emu / g. The coercive field (Hc) is about 641.83Oe. As the calcination temperature increases, the saturation magnetization (Ms) increases by 16.925emu / g, while the coercive field (Hc) decreases by 1639.47Oe. The trend of the change of magnetic parameters with the increase of calcination temperature is consistent with that of most ferrite ceramics. Instruction manual attached Figure 8 The hysteresis loops of L6S4FO (b) and L7S3FO (a) were tested after calcination at 1400℃ and annealing in an O2 environment at 800℃ for 6 hours. The saturation magnetization (Ms) of the L7S3FO sample calcined at 1400℃ is 60.463emu / g. The coercive field (Hc) is about 571.35Oe. As the substitution of the rare earth element La increases, the saturation magnetization (Ms) increases by 1.1emu / g, and the coercive force decreases by 70.48Oe. These magnetic parameters are comparable to those of pure SFO. The substitution of the earth element La does not significantly change the magnetic properties, but a new multiferroic material integrating FM and AFE is obtained.
[0063] La x Sr 1-x Fe 12 O 19The powder was pressed into cylindrical particles of Φ20×4nm. L6S4FO and L7S3FO were calcined at 1350℃ and 1400℃ for 2h respectively, and then annealed in 800℃ pure oxygen atmosphere in 3 steps for a total of 9 hours. The instrument used for the test was a UV-Vis-NIR spectrophotometer, which has a wavelength range of 200nm-2500nm, and can observe the spectrum more comprehensively and obtain more useful information. Fig. 9 The absorption spectra of L6S4FO (A) and L7S3FO (C) are shown. It can be seen that in the direction of shorter wavelengths, as the photon energy increases, the absorption coefficient increases sharply, and strong light absorption occurs, indicating the start of direct transition. It can be judged that the sample has obvious semiconductor properties and is a direct gap semiconductor. In the direction of shorter wavelengths, the first section is very flat and the absorption coefficient is very small because the intrinsically absorbed photoelectron energy is less than the bandgap width of the electron transition, and most of the electrons in the valence band do not obtain enough energy to transition to the conduction band. And because the photon energy is continuous, the electrons continue to absorb energy until it is greater than the bandgap width. At this time, as shown in the attached manual Fig. 9 A and instruction manual Fig. 9 The absorption coefficient shown in C increases sharply.
[0064] In order to calculate the bandgap of the sample, the absorption data is plotted (αE) 1 / n~ E, and then use the Tauc plot method to deduce the bandgap width. Since the sample is a direct gap semiconductor, n = 1 / 2. The formula is as follows
[0065] (αE) 2 =A(EE g )
[0066] When calculating Eg through Tauc plot, whether the absorption value or the absorption coefficient α is used, it actually has no effect on the Eg value. It is just that the coefficient A is different. Therefore, for simplicity, the absorption value can be directly used instead of α.
[0067] Instructions attached Fig. 9 (αE) of L6S4FO (B in the figure) and L7S3FO (D in the figure) 2~ Figure E, linear fitting is performed on the straight line parts of the figure, and then extrapolated to the horizontal axis. The intersection is the bandgap width. The bandgap widths of L6S4FO and L7S3FO are 1.741eV and 1.743eV respectively. The intrinsic absorption limits of both are in the infrared region, showing good semiconductor performance. As the substitution of La increases, the bandgap width increases slightly. Figure 1The shift of XRD diffraction peak can well explain this phenomenon. According to the Bragg equation 2dsinθ=nλ, as the substitution of La increases, the diffraction peak will shift slightly to the right, θ will increase, the interplanar spacing d will decrease, and the lattice constant will also decrease, thus increasing the binding force on electrons, requiring more energy for electrons to transition, and finally increasing the bandgap width.
[0068] Instructions attached Fig. 9 A and C are the absorption spectra of L6S4FO and L7S3FO calcined at 1350℃ and 1400℃ for 2h, respectively, and then annealed in 800℃ pure oxygen atmosphere in three steps for a total of 9 hours; B and D are the Taucplot (αE) of L6S4FO and L7S3FO, respectively. 2 Graph of the photon energy E as a function of the photon energy.
[0069] 4. La 0.6 Sr 0.4 Fe 12 O 19 Magnetoelectric Coupling Effect and Giant Magnetoresistance Effect of Ceramics
[0070] First, apply electrodes on both surfaces of the ceramic sample, place the sample in the middle of the mold and fix it in a plastic box. Then place the plastic box vertically between two electromagnets, and connect the electrodes to Keithley 2450Sourcemeter or Microtest 6630LCR for ME measurement. Turn on the electromagnet and increase the magnetic field with a gradient of 25mT from 25mT to 900mT, with a 30s interval between each gradient. Repeat the measurement many times, and the real part of the dielectric constant (ε') will show the following trend. Fig.10 The curves of dielectric constant changing with magnetic field at three frequencies are shown. When B is constant, the real part of dielectric constant gradually decreases with the increase of frequency. When the frequency is constant, when B<75mT, the real part of dielectric constant decreases with the increase of magnetic field. When B>75mT, the real part of dielectric constant increases nonlinearly with the increase of magnetic field. It can be seen that the magneto-dielectric response of dielectric performance modulated under the action of magnetic field changes greatly. When B=900mT and frequency is 500HZ, the change rate of real part of dielectric constant △ε' (△ε'={[(ε'(B)-ε'(0)] / ε'(0)}%) is 44%.
[0071] As the instruction manual Fig.11As shown, the function relationship between complex impedance and frequency under different magnetic fields (B) is shown, which is measured using Microtest 6630 LCR. Since the wires and electrodes of the capacitor have a certain resistivity, the dielectric has a certain dielectric loss. These losses are uniformly expressed as equivalent series resistance (ESR for short). The wires of the capacitor also have a certain inductance, which has a great influence at high frequencies and is expressed as equivalent series inductance (ESL for short). Therefore, the simplified equivalent circuit model of the capacitor is shown in the attached manual. Fig.12 As shown, it is drawn using AuToCAD. Based on this simplified model diagram, the complex impedance of the capacitor is calculated by the following formula
[0072]
[0073] The modulus of the complex impedance is calculated by
[0074]
[0075] From the instruction manual Fig.11 It can be seen that when the frequency is small (f<1.2MHz), the complex impedance decreases as the frequency increases. This is because at low frequencies, the inductive reactance is much smaller than the capacitive reactance. As the frequency increases, it can be seen from the complex impedance modulus calculation formula that the inductive reactance gradually increases, further offsetting the capacitive reactance, so that the complex impedance decreases as the frequency increases. The capacitor mainly exhibits capacitance in this low-frequency stage. When the frequency is 1.2MHz, the complex impedance is close to 0. This frequency point is the self-resonant frequency. At this frequency, the inductive reactance = the capacitive reactance, that is, At this time, the complex impedance is the smallest, showing pure resistance characteristics. When the frequency continues to increase (f>1.2MHz), the complex impedance begins to increase with the increase of frequency. This is because the inductive reactance begins to be greater than the capacitive reactance at high frequencies, causing the complex impedance to begin to increase. The capacitor mainly shows inductive properties at this high frequency stage. Fig.12 It can also be seen that the impedance gradually decreases with the increase of the magnetic field. When H=10Hz and B=0T, the resistance is 643Ω. When the magnetic field (B) gradually increases to 0.9T, the impedance decreases to 516Ω.
[0076] As the instruction manual Fig.13 As shown in the figure, the magnetic resistance ({(ZB-Z0) / ZB}%) of Z under different magnetic fields is shown. As the frequency increases (f<2.5Hz), MR tends to increase slightly. When the frequency is greater than 2.5KHz, MR increases sharply and reaches the maximum at around 20KHz. When B=0.9T and frequency is 20KHz, MR is -52.8%, which is not only much higher than that of a new material La under the same magnetic field, but also has a tendency to increase slightly. 0.9 Sr 0.1 The magnetoresistance of MnO3 is higher than that of NiFe / Cu three-layer alloy film (MR).
[0077] When the frequency continues to increase (f>20KHz), MR begins to decrease continuously. Fig.14 The functional relationship between the real part (Z') and the imaginary part (Z") of the complex impedance under different magnetic fields is shown. The real part (Z') and the imaginary part (Z") of the complex impedance form a classic Core-Core circle. The real part (Z') and the imaginary part (Z") of the complex impedance decrease with the increase of the magnetic field B, resulting in the radius of the cole-cole circle decreasing with the increase of B. As the applied magnetic field B increases from 0 to 0.9T, the real part decreases from 685Ω to 528Ω, and the imaginary part decreases from 239Ω to 177Ω. The real and imaginary parts change by 29.7% and 35%, respectively, at the magnetic field of B = 0.9T.
[0078] It is worth noting that higher giant magnetoresistance effects usually come from multilayer film systems. The magnetoelectric (ME) nanocomposite flexible film composed of electroactive polyvinylidene fluoride-hexafluoropropylene (P(VDF-HFP)) and ferromagnetic cobalt ferrite (CoFe2O4) has a giant magnetoresistance of about 15% near room temperature under the same magnetic field. However, the giant magnetoresistance of most bulk ceramics is very low. At room temperature, single-phase Zn x Fe 3-x The magnetic resistance of O4 is about 2%, and that of Zn 1-x Co x The magnetic reluctance of Fe2O4 ceramic ferrite is slightly less than 3%. 0.6 Sr 0.4 Fe 12 O 19 The giant magnetoresistance effect is very high among all current ceramic materials, even exceeding the giant magnetoresistance of some ferrite films.
[0079] V. Conclusion
[0080] By replacing SrFe with La ions 12 O 19 La formed by Sr ions in x Sr 1-x Fe 12 O 19 , the original FE state (x = 0) is transformed into the AFE state (x = 0.6), and the La substitution amount is further increased to transform into the PE state (x = 0.7). 0.6 Sr 0.4 Fe 12 O 19 The net macroscopic remnant polarization is almost zero, and the maximum value does not exceed 1.7uC / cm 2 , the PE loop shows an obvious double hysteresis loop in the high electric field region. The dielectric constant is abnormal near the Curie temperature. Both verify its inherent antiferroelectricity at room temperature. In addition, its energy density is 31.35J / cm 3, the energy storage efficiency is as high as 88.64%, exceeding most traditional perovskite ceramics. 0.6 Sr 0.4 Fe 12 O 19 ,La 0.7 Sr 0.3 Fe 12 O 19 Both compounds have the characteristics of magnetic semiconductors, with the calculated band gaps being 1.431eV and 1.743eV, the saturation magnetizations being 58.866emu / g and 60.463emu / g, and the coercive fields being 641.83Oe and 57.135Oe. 0.6 Sr 0.4 Fe 12 O 19 The compound also has magnetocapacitive effect and giant magnetoresistance effect. Under a 0.9T magnetic field, the dielectric constant increased by 44%, and the real part (Z') and imaginary part (Z") of the complex impedance increased by 29.7% and 35%, respectively. 0.6 Sr 0.4 Fe 12 O 19 The system is a new type of multiferroic candidate that combines AFE and FM and has magnetic semiconductor properties, magnetocapacitance effect and giant magnetoresistance effect.
[0081] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a rare earth substituted multiferroic M-type strontium lanthanum ferrite ceramic material, characterized in that: The following steps are involved: Step 1: Preparation of a first precursor: weigh 6 g of ferric acetylacetonate and dissolve it in 100 ml of acetone solvent, then pour it into a three-necked flask, and stir it at 70° C. for 6 hours in a glove box using a heating coil to obtain a first precursor; Step 2, preparation of the second precursor, weigh lanthanum acetate and strontium acetate according to the La: Sr: Fe molar ratio of 0.6: 0.4: 10, and then pour them into a single-necked flask filled with 15 ml of glycerol to dissolve and mix, and then distill the mixed solution in a rotary evaporator at 120 ° C for 2 hours, and transfer it to a 20 ml volumetric flask after it is completely dissolved, so as to obtain the second precursor; Step 3: Precursor mixing reaction: pour the second precursor into the three-necked flask containing the first precursor in the glove box in step 1, stir at 70°C for 6 hours, then add 60 ml of ammonia water to the precursor mixture, and react at 70°C for 24 hours to obtain a solution with particle precipitate; Step 4: After the precipitation is extracted, the three-necked flask with the precipitation is transferred to a centrifuge and centrifuged at 10,000 rpm for 15 minutes to remove the organic solvent to obtain precipitation particles, which are then calcined and ground twice to obtain single-phase hexaferrite. Nano powder; The two calcination treatments were calcination at 450°C for 1 hour followed by grinding for 30 minutes, then calcination at 800°C for 1 hour followed by grinding for 30 minutes, and then calcination at 750°C for 3 hours under oxygen conditions to remove organic impurities and nano-grinding to obtain single-phase hexaferrite. Step 5: Sample preparation and testing: weigh 0.06 g of single-phase hexaferrite nanopowder, press it into particles, sinter and anneal it to make a ceramic sample, and then use instruments to test the performance of the ceramic sample and record the test results; The specific preparation method of the ceramic pattern includes: S1. Weigh 0.06 g of single-phase hexaferrite nanopowder, press it into particles in a module and sinter it at 1350°C for 2 h to obtain a solid sample; S2, annealing the solid sample in a tube furnace at 800°C in a pure oxygen environment for 6 hours, then turning it over and continuing annealing for 6 hours, and then heat treating it in a high-temperature oxygen environment at 750°C for 3 hours to obtain a ceramic sample semi-finished product; S3. Silver paste is applied on both sides of the semi-finished ceramic pattern and cured at 820° C. for 15 minutes to form silver electrodes, thereby obtaining a finished ceramic pattern.
2. The method for preparing a rare earth substituted multiferroic M-type strontium lanthanum ferrite ceramic material according to claim 1, characterized in that: When the distilled solution is transferred to a 20 ml volumetric flask in the step 2, the small amount of solution remaining in the single-necked flask is rinsed with alcohol and poured into the volumetric flask. When the second precursor is poured into the three-necked flask in the step 3, the small amount of solution remaining in the volumetric flask is also rinsed with alcohol and poured into the three-necked flask.